Coal blending regulation and control method for preparing coke from biomass hydrothermal carbon

Through hydrothermal carbonization treatment of biomass and coal regulation, the premature reaction and dust emission problems in the blast furnace during the coking process are solved, efficient and low-pollution coke preparation is achieved, and the stability and energy of steel production are improved. Utilization efficiency.

CN118978928APending Publication Date: 2024-11-19ANSTEEL BEIJING RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411056410.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to effectively utilize biomass resources to prepare high-quality coke during the coking process, resulting in premature reactions in the blast furnace, increased dust emissions and low raw material utilization efficiency, and cannot meet the needs of blast furnace ironmaking production.

Method used

Through biomass hydrothermal carbonization treatment, biomass hydrothermal carbon with an alkali metal element content of less than 0.2%, was obtained, and mixed with various coal types to prepare and coordinate coal, adjust the Kirsch fluidity and colloidal layer thickness, and control the coking conditions to prepare efficient production , low-pollution coke.

Benefits of technology

It improves the energy utilization efficiency of the steel industry, reduces the emission of harmful substances, ensures the stability of coke quality and the stability of blast furnace production, reduces pretreatment energy consumption, and is suitable for a variety of energy and environmental applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978928A_ABST
    Figure CN118978928A_ABST
Patent Text Reader

Abstract

The invention relates to a coal blending regulation and control method for preparing coke from biomass hydrothermal carbon, which comprises the following steps: 1) carrying out hydrothermal carbonization treatment on a biomass raw material to obtain biomass hydrothermal carbon; the content of alkali metal elements in the biomass hydrothermal carbon is less than 0.2%; 2) preparing mixed coal: mixing multiple of gas coal, gas fat coal, coking coal, fat coal, 1 / 3 coking coal, lean coal and lean coking coal with the biomass hydrothermal carbon to form the mixed coal; the Gieseler fluidity G value of the blended coal is required to be 75-90 or the thickness Y value of a gelatinous layer is required to be 13.5-28mm; if the G value or the Y value does not meet the requirement, the G value and the Y value are adjusted by adjusting the type or proportion of pulverized coal or adding an additive; and 3) coking: coking the blended coal at the center temperature of a coking cake of 1250-1350 DEG C for 19-23 hours. On one hand, a correct biomass processing mode is provided, and on the other hand, the coal blending scheme is adjusted in time according to the type of biomass charcoal and the coal blending type.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coking, and in particular to a coal blending and regulating method for preparing coke from biomass hydrothermal charcoal. Background Art

[0002] As one of the main raw materials for ironmaking, coke accounts for more than 60% of the world's total coke production. Although my country is rich in coal resources, the regional distribution of coal resources is very uneven, and the regional differences in coal types are very large. High-quality coking coal resources for producing metallurgical coke for blast furnace ironmaking are even more scarce. China's steel production is mainly based on the blast furnace-converter long process, and blast furnace ironmaking production requires a large amount of metallurgical coke. The production and use of coke also emits a large amount of dust, nitrogen oxides, sulfur oxides and other pollutants, which leads to the continuous deterioration of the ecological environment and causes increasingly serious environmental problems.

[0003] Biomass energy is an environmentally friendly energy source. Biomass energy accounts for 10% to 14% of the world's primary energy. In the context of global energy resource shortage, it has important development potential and is also the only renewable carbon source. By 2050, depending on the source, biomass energy will account for more than 30% to 40% of the energy consumption structure. The application of biomass resources in coking production has become a hot topic in current research. In recent years, adding biomass-based fuels to blended coal to produce coke (also known as biocoke) has become a research hotspot. The ash content of biomass is low, usually 0.4 to 2.0wt.% (woody biomass), while the ash content of coal is about 10%. In addition, biomass contains alkaline components such as CaO and MgO, which can reduce the excessive dependence of blast furnace production on limestone to a certain extent. Compared with fossil fuel coal, the sulfur content in biomass-based fuels is much lower. Coke with biomass has a higher reactivity CRI and can be used as a substitute for coke, which helps to reduce the temperature of the thermal reserve area. However, the post-reaction strength CSR of coke with biomass is lower than that of ordinary coke, which has an adverse effect on the air and liquid permeability in the blast furnace. Studies have shown that the maximum amount of charcoal added to the mixed coal should be controlled within 5%. For crop-type biomass resources, affected by factors such as fertilization, when used as coking raw materials, the input of Na2O, K2O and P will increase, which will also have a certain impact on the reactivity of coke. Coke prepared with biomass-based fuels tends to react prematurely in the blast furnace, resulting in low efficiency of reducing agent utilization and increased dust emissions. Therefore, on the one hand, it is necessary to provide a correct way to handle biomass, and on the other hand, it is necessary to adjust the coal blending plan in time according to the type of biomass charcoal and the type of coal blending, so that the use of biomass in coking coal blending is more in line with the needs of blast furnace ironmaking production. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing coke from biomass hydrothermal charcoal.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for controlling coal blending for preparing coke from biomass hydrothermal charcoal, the specific steps comprising:

[0007] 1) The biomass raw material is subjected to hydrothermal carbonization treatment to obtain biomass hydrothermal carbon; the content of alkali metal elements in the biomass hydrothermal carbon is less than 0.2%;

[0008] 2) Preparation of blended coal: gas coal, gas fat coal, coking coal, fat coal, 1 / 3 coking coal, lean coal and lean coking coal are mixed with biomass hydrothermal charcoal to form blended coal; the Kiel fluidity G value of the blended coal is required to be 75-90 or the thickness Y value of the colloid layer is required to be 13.5-28 mm; if the G value or Y value does not meet the requirements, the G value and Y value are adjusted by adjusting the type or proportion of coal powder or adding additives;

[0009] 3) Coking: Coking is carried out with mixed coal, the center temperature of the coke cake is 1250-1350℃, and the coking time is 19-23h.

[0010] The biomass raw materials in step 1) include organic waste and energy plants. The organic waste includes agricultural waste, forestry waste and urban waste, and the energy plants include starch, cellulose and sugar.

[0011] Step 1) The hydrothermal carbonization treatment process: the biomass raw material is put into a high-pressure reactor, argon is introduced, the temperature is increased to 180-350°C at a rate of 10-20°C / min, and the temperature is kept at this temperature for 0.5-3h, followed by natural cooling. During the process, the material is stirred with a magnetic stirrer at 100-300rpm / min and the pressure is 5-30MPa.

[0012] Step 2) The mass ratio of biomass hydrothermal char in the blended coal is 1% to 10%.

[0013] Step 2) The additive is a binder or a slimming agent.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] On the one hand, the present invention provides a correct way to process biomass, and on the other hand, timely adjusts the coal blending scheme according to the type of biochar and the type of coal blending, so that the use of biomass in coking coal blending is more in line with the needs of blast furnace ironmaking production.

[0016] As a renewable energy source, the use of biomass hydrochar helps to improve the energy efficiency of the steel industry. By converting biomass into hydrochar, it can replace the use of some traditional fossil fuels, thereby reducing energy consumption and costs. The combustion process is relatively clean and can reduce the emission of harmful substances such as sulfur oxides and nitrogen oxides. This helps to improve the quality of the surrounding environment and meet the national requirements for environmental protection. Through coal blending and regulation schemes, the quality of coke can be ensured to be more stable, which is very important for the stability of steel production and product quality control. A stable supply of raw materials helps steel companies better plan production plans and reduce production risks caused by raw material fluctuations.

[0017] The key advantage of biomass hydrothermal carbonization to prepare coke is that it can efficiently convert biomass resources, and the produced coke has high energy density and calorific value, which is suitable for a variety of energy and environmental applications. Hydrothermal carbonization technology can directly process moist biomass raw materials at a lower temperature without the need for drying pretreatment. This feature greatly reduces the energy consumption of pretreatment and reduces the restrictions on raw material moisture. During the hydrothermal carbonization process, the physical and chemical properties of the resulting coke can be effectively adjusted by controlling different temperature and pressure conditions. When the HTC temperature exceeds 235°C, the fixed carbon ratio increases and the volatile matter ratio decreases, thereby increasing the calorific value of the coke. By adjusting the reaction conditions of hydrothermal carbonization (such as temperature, time), the physical and chemical properties of the coke can be customized to meet specific needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0020] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means more than two.

[0021] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0022] A method for controlling coal blending for preparing coke from biomass hydrothermal charcoal, the specific steps comprising:

[0023] 1) The biomass raw material is subjected to hydrothermal carbonization treatment to remove harmful alkali metal elements in the biomass raw material to obtain biomass hydrothermal carbon; the content of alkali metal elements in the biomass hydrothermal carbon is less than 0.2%;

[0024] 2) Preparation of blended coal: gas coal, gas fat coal, coking coal, fat coal, 1 / 3 coking coal, lean coal and lean coking coal are mixed with biomass hydrothermal charcoal to form blended coal; the Kiel fluidity G value of the blended coal is required to be 75-90 or the thickness of the colloid layer Y value is required to be 13.5-28 mm; if the G value or Y value does not meet the requirements, the G value and Y value are adjusted by adjusting the type or proportion of coal powder or adding a binder;

[0025] 3) Coking: Coking is carried out with mixed coal, the center temperature of the coke cake is 1250-1350℃, and the coking time is 19-23h.

[0026] The biomass raw materials in step 1) include organic waste and energy plants. The organic waste includes agricultural waste, forestry waste and urban waste, and the energy plants include starch, cellulose and sugar.

[0027] Step 1) The hydrothermal carbonization treatment process: the biomass raw material is put into a high-pressure reactor, argon is introduced, the temperature is increased to 180-350°C at a rate of 10-20°C / min, and the temperature is kept at this temperature for 0.5-3h, followed by natural cooling. During the process, the material is stirred with a magnetic stirrer at 100-300rpm / min and the pressure is 5-30MPa.

[0028] Step 2) The mass ratio of biomass hydrothermal char in the blended coal is 1% to 10%.

[0029] Step 2) The additive is a binder or a slimming agent.

[0030] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

[0031] In order to make the purpose, technical scheme and technical effect of the present invention clearer, the technical scheme in the embodiment of the present invention is now clearly and completely described. However, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. In combination with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] A method for controlling coal blending for preparing coke from biomass hydrothermal charcoal, a laboratory-scale small-scale coking method, and the specific steps include:

[0034] 1) Hydrothermal carbonization of biomass: corn stalks were ball-milled and then added with water and placed in a high-pressure reactor for heating, with 40-50g of solid and 200-300ml of liquid. Heating system: 25℃ to target temperature 300℃, heating rate 2.5℃ / min; insulation process: target temperature 300℃, insulation 60min; cooling process: natural cooling, using pressure 15Mpa, using gas: high-purity argon, and propeller stirring during the experiment. Take out the solid and dry it to obtain biomass hydrothermal carbon.

[0035] 2) Prepare blended coal: gas coal, gas fat coal, coking coal, fat coal, 1 / 3 coking coal, lean coal, and lean coking coal are mixed with biomass hydrothermal charcoal to form blended coal. The specific mass percentage of the blended coal components is: biomass hydrothermal charcoal: 5%, coking coal: 50%, 1 / 3 coking coal: 15%, fat coal: 15%, and lean coal: 15%. The Kiel fluidity G value of the blended coal is required to be 75-90 or the gelatin layer thickness Y value is 13.5-28mm;

[0036] 3) Performance testing of blended coal

[0037] The properties of the blended coal were tested, including the active-inert ratio, the Kiel fluidity G value or the colloidal layer thickness Y value of the coking coal, etc. The test results using laboratory testing equipment were: active-inert ratio <4, G value 72, Y value 17.5;

[0038] The G value and Y value can be adjusted by adjusting the type or proportion of coal powder or adding a binder. In this embodiment, 2% of a binder (coal tar) is added. After adjustment, the G value of the coking coal is 83 or the Y value is 19.7 mm.

[0039] 4) Coking

[0040] The coking coal is used for coking, the center temperature of the coke cake is 1300℃ and the coking time is 20h.

[0041] 5) Coke quality inspection

[0042] The coke quality testing process is to test the coke reactivity CRI and coke post-reaction strength CSR according to the national standard GBT 4000-2017. The test results are CRI is 27% and CSR is 64%, which meets the production requirements.

[0043] Example 2

[0044] A method for controlling coal blending for preparing coke from biomass hydrothermal charcoal, the specific steps comprising:

[0045] 1) Hydrothermal carbonization of biomass

[0046] A large-scale high-pressure reactor of a manufacturing enterprise is used, with a capacity of 100 kg. After ball milling, corn stalks are added with water and placed in a high-pressure reactor for heating, with 40-50 kg of solid and 200-300 L of liquid. The heating system is from 25°C to the target temperature of 300°C, with a heating rate of 2°C / min; the heat preservation process is the target temperature of 300°C, and the heat preservation is 120 minutes; the cooling process is natural cooling, the pressure used is about 15Mpa, and the gas used is high-purity argon. During the experiment, the equipment's own propeller can be used for stirring. The solid part taken out is processed by a large-scale continuous drying equipment to obtain a large amount of biomass hydrothermal charcoal.

[0047] 2) Preparation of blended coal

[0048] According to the needs of industrial production, the mixing ratio of single coal and biomass hydrochar is increased proportionally, keeping the mass percentage unchanged. Multiple single coals from gas coal, gas fat coal, coking coal, fat coal, 1 / 3 coking coal, lean coal, and lean coking coal are mixed with biomass hydrochar to form blended coal. The specific mass percentages of the blended coal components are: biomass hydrochar: 5%, coking coal: 50%, 1 / 3 coking coal: 15%, fat coal: 15%, and lean coal: 15%. The Kiel fluidity G value of the blended coal is required to be 75-90 or the gelatin layer thickness Y value is 13.5-28mm; mix in a mixer to ensure that the mixture is uniform.

[0049] 3) Performance testing of blended coal

[0050] The properties of the blended coal were tested, including the active-inert ratio, Kielder fluidity G value and colloidal layer thickness Y value. The test results were: active-inert ratio <4, G value 75, Y value 18.1; meeting the requirements;

[0051] The G value and Y value can be adjusted by adjusting the type or proportion of coal powder or adding a binder; in this embodiment, 2% of a binder (asphalt) is added. After adjustment, the G value of the coking coal is 81.3 or the Y value is 18.9 mm;

[0052] 4) Coking

[0053] Industrial coking furnaces are used for coking, and the coking time and temperature are adjusted according to the actual equipment and production conditions. The maximum heating temperature is set between 1300℃ and 1400℃, and the heat preservation at the highest temperature is 15 hours.

[0054] 5) Coke quality inspection

[0055] Coke quality testing was carried out according to the relevant national standards, such as GBT 4000-2017. The coke reactivity CRI and coke post-reaction strength CSR were tested. The test results showed that the CRI was 26.4% and the CSR was 62%, which met the production requirements.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for controlling coal blending in preparing coke from biomass hydrothermal charcoal, characterized in that: The specific steps include: 1) The biomass raw material is subjected to hydrothermal carbonization treatment to obtain biomass hydrothermal carbon; the content of alkali metal elements in the biomass hydrothermal carbon is less than 0.2%; 2) Preparation of blended coal: gas coal, gas fat coal, coking coal, fat coal, 1 / 3 coking coal, lean coal and lean coking coal are mixed with biomass hydrothermal charcoal to form blended coal; the Kiel fluidity G value of the blended coal is required to be 75-90 or the thickness Y value of the colloid layer is required to be 13.5-28 mm; if the G value or Y value does not meet the requirements, the G value and Y value are adjusted by adjusting the type or proportion of coal powder or adding additives; 3) Coking: Coking is carried out with mixed coal, the center temperature of the coke cake is 1250-1350℃, and the coking time is 19-23h.

2. The method for controlling coal blending for preparing coke from biomass hydrothermal charcoal according to claim 1, characterized in that: The biomass raw materials in step 1) include organic waste and energy plants. The organic waste includes agricultural waste, forestry waste and urban waste, and the energy plants include starch, cellulose and sugar.

3. The method for controlling coal blending for preparing coke from biomass hydrothermal charcoal according to claim 1, characterized in that: Step 1) The hydrothermal carbonization treatment process: the biomass raw material is put into a high-pressure reactor, argon is introduced, the temperature is increased to 180-350°C at a rate of 10-20°C / min, and the temperature is kept at this temperature for 0.5-3h, followed by natural cooling. During the process, the material is stirred with a magnetic stirrer at 100-300rpm / min and the pressure is 5-30MPa.

4. The method for controlling coal blending for preparing coke from biomass hydrothermal charcoal according to claim 1, characterized in that: Step 2) The mass ratio of biomass hydrothermal char in the blended coal is 1% to 10%.

5. The method for controlling coal blending for preparing coke from biomass hydrothermal charcoal according to claim 1, characterized in that: Step 2) The additive is a binder or a slimming agent.