Coated windshield washer fluid as well as preparation method and application thereof

By adding composite sol to the automotive glass water, using the combination of silicate particles and modified nano titanium dioxide, the problem of poor decontamination effect of existing automotive glass water is solved, and efficient decontamination and multi-functional coated glass water is achieved, suitable for a wide range of applications. use.

CN118978963APending Publication Date: 2024-11-19JIAXING CHENGKAI ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411060954.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing automobile glass has a single function and poor decontamination and cleaning effect. It is difficult to effectively remove organic matter such as insect corpses, bird droppings, oil and other organic matter on the glass during driving, affecting driving vision.

Method used

Develop a coated glass water to form fine silicate particles and modified nanotitanium dioxide to the glass water to achieve optical cleaning and physical Cleansing, quickly removes stains and breaks down organic matter.

Benefits of technology

It realizes efficient decontamination, anti-freeze, anti-fog, anti-static and other functions, which are safe and environmentally friendly, non-corrosion, low-cost, and suitable for promotion and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004977834330000071
    Figure BDA0004977834330000071
Patent Text Reader

Abstract

The invention belongs to the technical field of automobile glass cleaning agents, and discloses coated glass water as well as a preparation method and application thereof. The coated glass water is prepared from ethylene glycol, sodium dodecyl benzene sulfonate, a penetrating agent, an emulsifying agent, a defoaming agent, a corrosion inhibitor, composite sol, ethyl alcohol and water, and the composite sol is prepared from tetraethyl orthosilicate, nanometer titania, sodium carboxymethyl cellulose and zinc stannate nanometer microspheres. The coated glass water prepared by the invention has both optical cleaning effect and physical cleaning effect, is efficient in decontamination, does not damage automobile glass, and is simple in preparation process, low in raw material price and suitable for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of automobile glass cleaners, and in particular to a coated glass water, a preparation method and an application thereof. Background Art

[0002] As the number of cars in the market increases, the cleanliness and beauty of car glass and the good vision of the driver during driving are also one of the issues that people focus on in daily life. After a long period of driving, due to the influence of external environment such as wind, sun and rain, a large amount of dust and dirt will often be deposited on the car glass. If it is not cleaned up in time, it will not only affect the overall appearance of the car, but also interfere with the driver's vision. Therefore, keeping the glass clean and bright during the use of the car has become the focus of attention of every motor vehicle driver. Although there are many varieties of existing car glass water, they often have single functions and poor decontamination and cleaning effects. Organic matter such as insect corpses, bird droppings, and oil stains during driving are stained on the glass, which can easily cause blurred vision after being smeared by the wiper. Therefore, it is necessary to develop a self-cleaning function that can effectively decompose the organic matter on the car glass or dissolve the organic matter on the car glass, or can remove the organic matter on the car glass through physical action. Summary of the invention

[0003] In order to solve the above technical problems, an efficient decontamination glass water with both optical cleaning and physical cleaning effects, good cleaning effect and no damage to automobile glass is developed. The present application provides a coated glass water, a preparation method and an application.

[0004] In the first aspect, the present application provides a coated glass water, comprising the following raw materials in parts by weight: 6-14 parts of ethylene glycol, 4-7 parts of sodium dodecylbenzene sulfonate, 3-5 parts of penetrant, 2-4 parts of emulsifier, 2-4 parts of defoamer, 2-3 parts of corrosion inhibitor, 22-40 parts of composite sol, 18-35 parts of ethanol, and 200-350 parts of water; the raw materials of the composite sol include tetraethyl orthosilicate, nano titanium dioxide, sodium carboxymethyl cellulose and zinc stannate nano microspheres.

[0005] By adopting the above technical scheme, the tetraethyl orthosilicate in the present application undergoes a hydrolysis reaction under acidic conditions to generate silanols. When the silanols are sprayed onto the vehicle glass surface along with the glass water, they easily react to form fine silicate particles, so that the wiper rubber strip can rub and scrape off the stains adhered to the glass surface under the friction of the fine silicate particles. At the same time, the fine silicate particles are directly converted from liquid molecules to solid particles, and the generation speed is relatively slow. Therefore, in the short time from spraying the glass water onto the vehicle glass surface to the wiper rubber strip scraping away the glass water, the silicate particles formed are small and uniform in size, and the number is small, so that the silicate particles cannot aggregate and grow, thereby avoiding the problem of silicate particles scratching the car glass. In addition, the nano-titanium dioxide in the composite sol acts as a photocatalyst and can decompose organic matter on the surface of the glass under light conditions. In the present application, zinc stannate nano-microspheres are used to modify the nano-titanium dioxide, which can improve the absorption capacity of nano-titanium dioxide and even infrared light, expand the visible light response, inhibit the recombination of photogenerated electrons and holes, and increase the surface hydroxyl radical content, thereby promoting the decomposition of organic matter on the surface of automotive glass.

[0006] Preferably, the coated glass water comprises the following raw materials in parts by weight: 8 parts of ethylene glycol, 6.5 parts of sodium dodecylbenzene sulfonate, 3.5 parts of penetrant, 2-4 parts of emulsifier, 2-4 parts of defoamer, 2-3 parts of corrosion inhibitor, 36 parts of composite sol, 30 parts of ethanol, and 300 parts of water.

[0007] By adopting the above technical solution, the coated glass water prepared by the above ratio can fully combine the optical cleaning effect and the physical cleaning effect, and perform efficient decontamination without damaging the automobile glass.

[0008] Furthermore, the penetrant includes one or more of fatty alcohol polyoxyethylene ether, polyethylene glycol, and diisooctyl maleate sulfonate.

[0009] Furthermore, the defoaming agent includes one or more of glycerol, polyether-modified siloxane, and dimethyl silicone oil.

[0010] Furthermore, the composite sol comprises tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres, and nano-titanium dioxide in a weight ratio of 5-8:12-20:0.3-0.6:0.1-0.15:0.7-1.2.

[0011] Preferably, the composite sol comprises tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres, and nano-titanium dioxide in a weight ratio of 7:16:0.5:0.12:1.

[0012] Furthermore, the preparation method of the composite sol includes the following steps: adding tetraethyl orthosilicate and water into a reaction container, adjusting the pH, stirring at 40°C until the liquid is clear and transparent, adding sodium carboxymethyl cellulose and modified nano titanium dioxide, ultrasonically dispersing at 60°C, cooling, and standing to obtain a composite sol.

[0013] Preferably, the preparation method of the composite sol comprises the following steps: adding tetraethyl orthosilicate and water into a reaction container, adjusting the pH to 2-3, stirring at 40°C until the liquid becomes clear and transparent, adding sodium carboxymethyl cellulose and modified nano titanium dioxide, ultrasonically dispersing at 60°C for 15 minutes, cooling to 25°C, and standing for 2 hours to obtain a composite sol.

[0014] Furthermore, the preparation method of the modified nano titanium dioxide comprises the following steps: adding nano titanium dioxide to water, ultrasonicating at 30-50°C, adding a surface modifier, ultrasonicating, adding a coupling agent, ultrasonicating, adding zinc stannate nano microspheres, ultrasonicating, filtering, and drying to obtain modified nano titanium dioxide.

[0015] Preferably, the preparation method of the modified nano titanium dioxide comprises the following steps: adding nano titanium dioxide to water, the mass fraction of nano titanium dioxide is 10%, ultrasonicating at 50°C for 10 minutes, adding a surface modifier, ultrasonicating for 15 minutes, adding a coupling agent, ultrasonicating for 10 minutes, adding zinc stannate nano microspheres, ultrasonicating for 25 minutes, filtering, drying, and obtaining modified nano titanium dioxide. Among them, the surface modifier is octadecyl quaternary ammonium salt, and the coupling agent is a silane coupling agent. The weight ratio of nano titanium dioxide, surface modifier and coupling agent is 1:0.03:0.02.

[0016] In a second aspect, the present application provides a method for preparing the above-mentioned coated glass water, comprising the following steps: S1, taking the above raw materials according to the ratio, mixing the composite sol, ethanol and water, placing in a water bath oscillator, and oscillating to obtain a mixture A; S2. Add the remaining raw materials into mixture A, ultrasonicate and stir to obtain coated glass water.

[0017] Preferably, in step S1, the water bath oscillation temperature is set to 30-40° C., the oscillation frequency is 15-30 r / min, the oscillation time is 20-30 min, and the oscillation is performed in a protective gas atmosphere.

[0018] On the third aspect, the present application provides the application of the above-mentioned coated glass water in the field of automobile glass and household glass cleaning.

[0019] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The coated glass water provided in this application has good decontamination and cleaning effect, can quickly remove stains such as oil, shellac, dust, etc. on the windshield, is low in cost, has multiple functions such as antifreeze, anti-fog, anti-static, etc., is safe, environmentally friendly and non-corrosive.

[0020] 2. The coated glass water provided in this application has both optical cleaning and physical cleaning effects, can remove dirt efficiently without damaging automobile glass, has a simple preparation process, and has low raw material prices, making it suitable for popularization and use. DETAILED DESCRIPTION

[0021] The present application designs a coated glass water, which comprises the following raw materials in parts by weight: 6-14 parts of ethylene glycol, 4-7 parts of sodium dodecylbenzene sulfonate, 3-5 parts of penetrant, 2-4 parts of emulsifier, 2-4 parts of defoamer, 2-3 parts of corrosion inhibitor, 22-40 parts of composite sol, 18-35 parts of ethanol, and 200-350 parts of water; the raw materials of the composite sol include tetraethyl orthosilicate, nano titanium dioxide, sodium carboxymethyl cellulose and zinc stannate nano microspheres.

[0022] The preparation method of the composite sol comprises the following steps: adding tetraethyl orthosilicate and water into a reaction container, adjusting pH, stirring at 40°C until the liquid is clear and transparent, adding sodium carboxymethyl cellulose and modified nano titanium dioxide, ultrasonically dispersing at 60°C, cooling, and standing to obtain the composite sol.

[0023] The preparation method of modified nano titanium dioxide comprises the following steps: adding nano titanium dioxide into water, ultrasonicating at 30-50° C., adding a surface modifier, ultrasonicating, adding a coupling agent, ultrasonicating, adding zinc stannate nano microspheres, ultrasonicating, filtering, and drying to obtain modified nano titanium dioxide.

[0024] The coated glass water of the present application is prepared by the following method, comprising the following steps: S1, taking the above raw materials according to the ratio, mixing the composite sol, ethanol and water, placing in a water bath oscillator, and oscillating to obtain a mixture A; S2. Add the remaining raw materials into mixture A, ultrasonicate and stir to obtain coated glass water.

[0025] The coated glass water of the present application can be used in the fields of automobile glass and household glass cleaning.

[0026] The technical problem solved by the present application is that although the existing automobile windshield water has a wide variety of varieties, it often has a single function and poor decontamination and cleaning effect. During driving, organic matter such as insect corpses, bird droppings, and oil stains are stained on the glass, which can easily cause blurred vision after being smeared by the wiper. The present application adds a composite sol containing specific components to conventional glass water to prepare a coated glass water that has both optical cleaning and physical cleaning effects, high-efficiency decontamination without damaging automobile glass, and can quickly remove stains such as oil, shellac, and dust on the windshield. It is low in cost and has multiple functions such as antifreeze, anti-fog, and anti-static. The preparation process is simple and the raw material price is low, which is suitable for promotion and use.

[0027] The present application is further described in detail below in conjunction with specific embodiments.

[0028] Examples 1-5 The coated glass water prepared in Example 1 includes the following raw materials in parts by weight: 22 parts of composite sol, 8 parts of ethylene glycol, 6.5 parts of sodium dodecylbenzene sulfonate, 3.5 parts of penetrant, 3 parts of emulsifier, 3 parts of defoamer, 2.5 parts of corrosion inhibitor, 30 parts of ethanol, and 300 parts of water.

[0029] The coated glass water prepared in Example 2 includes the following raw materials in parts by weight: 36 parts of composite sol, 8 parts of ethylene glycol, 6.5 parts of sodium dodecylbenzene sulfonate, 3.5 parts of penetrant, 3 parts of emulsifier, 3 parts of defoamer, 2.5 parts of corrosion inhibitor, 30 parts of ethanol, and 300 parts of water.

[0030] The coated glass water prepared in Example 3 includes the following raw materials in parts by weight: 40 parts of composite sol, 8 parts of ethylene glycol, 6.5 parts of sodium dodecylbenzene sulfonate, 3.5 parts of penetrant, 3 parts of emulsifier, 3 parts of defoamer, 2.5 parts of corrosion inhibitor, 30 parts of ethanol, and 300 parts of water.

[0031] The coated glass water prepared in Example 4 includes the following raw materials in parts by weight: 36 parts of composite sol, 6 parts of ethylene glycol, 7 parts of sodium dodecylbenzene sulfonate, 3 parts of penetrant, 2 parts of emulsifier, 2 parts of defoamer, 2 parts of corrosion inhibitor, 18 parts of ethanol, and 200 parts of water.

[0032] The coated glass water prepared in Example 5 includes the following raw materials in parts by weight: 36 parts of composite sol, 14 parts of ethylene glycol, 4 parts of sodium dodecylbenzene sulfonate, 5 parts of penetrant, 4 parts of emulsifier, 4 parts of defoamer, 3 parts of corrosion inhibitor, 35 parts of ethanol, and 350 parts of water.

[0033] The penetrant used in Examples 1-5 is fatty alcohol polyoxyethylene ether, model AEO-7.

[0034] The emulsifier used in Examples 1-5 is Triton X-165.

[0035] The defoaming agent used in Examples 1-5 is dimethyl silicone oil.

[0036] The corrosion inhibitor used in Examples 1-5 is methylbenzotriazole.

[0037] The preparation process of the composite sol used in Examples 1-5 comprises the following steps: (1) Add nano titanium dioxide to water, the mass fraction of nano titanium dioxide is 10%, ultrasonicate for 10 minutes at 50°C, add a surface modifier, ultrasonicate for 15 minutes, add a coupling agent, ultrasonicate for 10 minutes, add zinc stannate nano microspheres, ultrasonicate for 25 minutes, filter, dry, and obtain modified nano titanium dioxide. The surface modifier is octadecyl quaternary ammonium salt, the coupling agent is silane coupling agent KH560; the amount of the surface modifier is 3wt% of the nano titanium dioxide, and the amount of the coupling agent is 2wt% of the nano titanium dioxide.

[0038] (2) Add tetraethyl orthosilicate and water to a reaction container, adjust the pH to 2-3, stir at 40° C. until the liquid becomes clear and transparent, add sodium carboxymethyl cellulose and the modified nano-titanium dioxide prepared in step (1), ultrasonically disperse at 60° C. for 15 min, cool to 25° C., and stand for 2 h to obtain a composite sol.

[0039] In step (1) and step (2), the weight ratio of tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres, and nano-titanium dioxide is 7:16:0.5:0.12:1.

[0040] The method for preparing the coated glass water in Examples 1-5 comprises the following steps: S1. Take the above raw materials according to the ratio, mix the composite sol, ethanol and water, and place them in a water bath oscillator. The water bath oscillation temperature is set to 30° C., the oscillation frequency is 25 r / min, and the mixture is shaken in a nitrogen atmosphere for 22 minutes to obtain a mixture A; S2. Add the remaining raw materials to mixture A, ultrasonicate for 20 minutes, and stir for 10 minutes to obtain coated glass water.

[0041] Example 6 Example 6 is based on Example 2, except that the permeation agent used in Example 6 is changed to polyethylene glycol.

[0042] The method for preparing the coated glass water in Example 6 comprises the following steps: S1. Take the above raw materials according to the ratio, mix the composite sol, ethanol and water, and place them in a water bath oscillator. The water bath oscillation temperature is set to 30° C., the oscillation frequency is 25 r / min, and the mixture is shaken in a nitrogen atmosphere for 22 minutes to obtain a mixture A; S2. Add the remaining raw materials to mixture A, ultrasonicate for 20 minutes, and stir for 10 minutes to obtain coated glass water.

[0043] Embodiment 7-8 Example 7 is based on Example 2, except that the weight ratio of the raw materials of the composite sol in Example 7, tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres, and nano-titanium dioxide, is changed to: 5:12:0.3:0.1:1.2.

[0044] Example 8 is based on Example 2, except that the weight ratio of the raw materials of the composite sol in Example 8, tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres, and nano-titanium dioxide, is changed to: 8:20:0.6:0.15:0.7.

[0045] The method for preparing the coated glass water in Examples 7-8 comprises the following steps: S1. Take the above raw materials according to the ratio, mix the composite sol, ethanol and water, and place them in a water bath oscillator. The water bath oscillation temperature is set to 30° C., the oscillation frequency is 25 r / min, and the mixture is shaken in a nitrogen atmosphere for 22 minutes to obtain a mixture A; S2. Add the remaining raw materials to mixture A, ultrasonicate for 20 minutes, and stir for 10 minutes to obtain coated glass water.

[0046] Comparative Example 1 Comparative Example 1 is based on Example 2, except that: zinc stannate nanoparticles are not added when preparing the composite sol in Comparative Example 1. That is, the preparation process of the composite sol in Comparative Example 1 includes the following steps: (1) Add nano titanium dioxide to water, the mass fraction of nano titanium dioxide is 10%, ultrasonicate for 10 minutes at 50°C, add a surface modifier, ultrasonicate for 15 minutes, add a coupling agent, ultrasonicate for 10 minutes, ultrasonicate for 25 minutes, filter, dry, and obtain modified nano titanium dioxide. The surface modifier is octadecyl quaternary ammonium salt, and the coupling agent is silane coupling agent KH560; the amount of the surface modifier is 3wt% of the nano titanium dioxide, and the amount of the coupling agent is 2wt% of the nano titanium dioxide.

[0047] (2) Add tetraethyl orthosilicate and water to a reaction container, adjust the pH to 2-3, stir at 40° C. until the liquid becomes clear and transparent, add sodium carboxymethyl cellulose and the modified nano-titanium dioxide prepared in step (1), ultrasonically disperse at 60° C. for 15 min, cool to 25° C., and stand for 2 h to obtain a composite sol.

[0048] In step (1) and step (2), the weight ratio of tetraethyl orthosilicate, water, sodium carboxymethyl cellulose and nano titanium dioxide is 7:16:0.5:1.

[0049] Comparative Example 2 Comparative Example 2 is based on Example 2, except that when preparing the composite sol in Comparative Example 2, an equal amount of nano-titanium dioxide is replaced by nano-silicon dioxide.

[0050] The preparation process of the composite sol used in Comparative Example 2 comprises the following steps: (1) Add nano-silicon dioxide to water, the mass fraction of nano-silicon dioxide is 10%, ultrasonicate for 10 minutes at 50°C, add a surface modifier, ultrasonicate for 15 minutes, add a coupling agent, ultrasonicate for 10 minutes, add zinc stannate nano-microspheres, ultrasonicate for 25 minutes, filter, dry, and obtain modified nano-silicon dioxide. The surface modifier is octadecyl quaternary ammonium salt, the coupling agent is silane coupling agent KH560; the amount of the surface modifier is 3wt% of the nano-silicon dioxide, and the amount of the coupling agent is 2wt% of the nano-silicon dioxide.

[0051] (2) Add tetraethyl orthosilicate and water to a reaction container, adjust the pH to 2-3, stir at 40° C. until the liquid becomes clear and transparent, add sodium carboxymethyl cellulose and the modified nano-silica prepared in step (1), ultrasonically disperse at 60° C. for 15 min, cool to 25° C., and stand for 2 h to obtain a composite sol.

[0052] In step (1) and step (2), the weight ratio of tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres, and nano-silicon dioxide is 7:16:0.5:0.12:1.

[0053] The preparation method of the coated glass water in Comparative Example 2 comprises the following steps: S1. Take the above raw materials according to the ratio, mix the composite sol, ethanol and water, and place them in a water bath oscillator. The water bath oscillation temperature is set to 30° C., the oscillation frequency is 25 r / min, and the mixture is shaken in a nitrogen atmosphere for 22 minutes to obtain a mixture A; S2. Add the remaining raw materials to mixture A, ultrasonicate for 20 minutes, and stir for 10 minutes to obtain coated glass water.

[0054] Performance measurement 1. The freezing point (°C) and metal corrosion (for galvanized steel sheets) of the coated glass water prepared in Examples 1-8 and Comparative Examples 1-2 were measured respectively.

[0055] 2. Refer to the method in standard GB / T23436-2009 to test the cleaning power of windshield washer fluid in light and dark environments, and record the number of reciprocating scraping times of the wiper and whether there is any dirt residue when using windshield washer fluid for cleaning.

[0056] The measurement results are shown in Table 1.

[0057] Table 1 By analyzing the data in Table 1 and comparing the performance data of the coated glass water in Examples 1-8 with those in Comparative Examples 1-2, it can be found that zinc stannate nano-microspheres and titanium dioxide have a significant effect on the decontamination and anti-corrosion effects of the coated glass water in this application.

[0058] The coated glass water prepared in the present application has good decontamination and cleaning effect, can quickly remove stains on the windshield, has good antifreeze performance, is safe, environmentally friendly and non-corrosive.

[0059] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A coated glass water, characterized in that: The invention comprises the following raw materials in parts by weight: 6-14 parts of ethylene glycol, 4-7 parts of sodium dodecylbenzene sulfonate, 3-5 parts of penetrant, 2-4 parts of emulsifier, 2-4 parts of defoamer, 2-3 parts of corrosion inhibitor, 22-40 parts of composite sol, 18-35 parts of ethanol and 200-350 parts of water; The raw materials of the composite sol include tetraethyl orthosilicate, nano titanium dioxide, sodium carboxymethyl cellulose and zinc stannate nano microspheres.

2. The coated glass water according to claim 1, characterized in that: The coated glass water comprises the following raw materials in parts by weight: 8 parts of ethylene glycol, 6.5 parts of sodium dodecylbenzene sulfonate, 3.5 parts of penetrant, 2-4 parts of emulsifier, 2-4 parts of defoamer, 2-3 parts of corrosion inhibitor, 36 parts of composite sol, 30 parts of ethanol and 300 parts of water.

3. The coated glass water according to claim 1, characterized in that: The penetrant includes one or more of fatty alcohol polyoxyethylene ether, polyethylene glycol, and diisooctyl maleate sulfonate.

4. The coated glass water according to claim 1, characterized in that: The defoaming agent includes one or more of glycerol, polyether-modified siloxane and dimethyl silicone oil.

5. The coated glass water according to claim 1, characterized in that: The raw materials of the composite sol include tetraethyl orthosilicate, water, sodium carboxymethyl cellulose, zinc stannate nano-microspheres and nano-titanium dioxide in a weight ratio of 5-8:12-20:0.3-0.6:0.1-0.15:0.7-1.

2.

6. The coated glass water according to claim 1, characterized in that: The preparation method of the composite sol comprises the following steps: adding tetraethyl orthosilicate and water into a reaction container, adjusting pH, stirring at 40°C until the liquid is clear and transparent, adding sodium carboxymethyl cellulose and modified nano titanium dioxide, ultrasonically dispersing at 60°C, cooling, and standing to obtain the composite sol.

7. The coated glass water according to claim 6, characterized in that: The preparation method of modified nano titanium dioxide comprises the following steps: adding nano titanium dioxide into water, ultrasonicating at 30-50° C., adding a surface modifier, ultrasonicating, adding a coupling agent, ultrasonicating, adding zinc stannate nano microspheres, ultrasonicating, filtering, and drying to obtain modified nano titanium dioxide.

8. A method for preparing coated glass water according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, taking the above raw materials according to the ratio, mixing the composite sol, ethanol and water, placing in a water bath oscillator, and oscillating to obtain a mixture A; S2. Add the remaining raw materials into mixture A, ultrasonicate and stir to obtain coated glass water.

9. Use of the coated glass water according to any one of claims 1 to 7 in cleaning automobile glass and household glass.