High-hardness hard alloy drawing die material and preparation method thereof
By using multi-layer structure and wear-resistant layer technology in cemented carbide drawing molds, combined with multi-component collaboration and injection molding processes, the problem of difficult to improve the inner surface hardness and overall toughness of the mold in the prior art is solved, and high The mold design of hardness, toughness and fatigue resistance extends the service life of the mold.
Patent Information
- Application Number
- CN202411058523.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to simultaneously improve the inner surface hardness and overall toughness of cemented carbide drawing molds, resulting in the mold being easily fatigued or cracked and failed after long-term service, especially under high temperature conditions.
By mixing tungsten carbide powder, cobalt powder, cobalt aluminum-tungsten high-temperature alloy powder and cobalt nickel-molybdenum three-main alloy powder in a certain proportion, cold forming and pneumatic sintering are carried out to form a multi-layer structure cemented carbide drawing mold, and A wear-resistant layer is deposited on the inner surface of the mold, and a solid metallurgical bonding interface is formed using multi-component synergy and injection molding technology.
The high hardness, toughness and fatigue resistance of cemented carbide drawing molds are achieved, ensuring the dimensional accuracy and service life of the mold, and avoiding fatigue or cracking problems caused by interlayer stress concentration.
Smart Images

Figure BDA0004977113310000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cemented carbide drawing die preparation, and in particular relates to a high-hardness cemented carbide drawing die material and a preparation method thereof. Background Art
[0002] Cemented carbide drawing dies are mainly used for drawing plastic metal wires. The inner surface hardness and overall toughness have an impact on the surface roughness, dimensional accuracy, and processing efficiency and life of the drawing materials. Common methods to improve the surface hardness of cemented carbide drawing dies are inner surface coating technology, adjusting the cobalt phase content, and ladle cemented carbide methods.
[0003] Inner surface coating technology, due to the large performance difference between the harder surface layer and the cemented carbide substrate, it is easy to cause the coating to fall off prematurely, making the wear-resistant layer ineffective;
[0004] Adjusting the cobalt phase content is another conventional means to change the hardness and toughness properties of cemented carbide, but the "inverted" relationship between hardness and toughness changes significantly with the cobalt content, making it difficult to meet the dual requirements of hardness and toughness of drawing dies;
[0005] The ladle carbide method can combine the toughness of steel and the hardness of carbide, balancing the relationship between hardness and toughness to a certain extent. However, under long-term service, especially under high temperature conditions, the ladle sleeve is prone to softening and fatigue, causing the carbide core to crack, resulting in mold failure.
[0006] Therefore, the commonly used inner surface coating technology, adjusting the cobalt phase content and ladle cemented carbide methods are difficult to simultaneously improve the inner surface hardness, overall toughness and service life of cemented carbide drawing dies. Summary of the invention
[0007] The purpose of the present invention is to provide a high-hardness cemented carbide drawing die material and a preparation method thereof, which solves the engineering problem that the existing method is difficult to simultaneously improve the inner surface hardness and overall toughness of the cemented carbide drawing die.
[0008] The present invention is achieved through the following technical solutions:
[0009] A method for preparing a high-hardness cemented carbide drawing die material comprises the following steps:
[0010] 1) mixing tungsten carbide powder and cobalt powder to obtain mixed powder A;
[0011] Mix tungsten carbide powder and cobalt-aluminum-tungsten high-temperature alloy powder to obtain mixed powder B;
[0012] Mixing tungsten carbide powder with cobalt, nickel and molybdenum three-element alloy powder to obtain mixed powder C;
[0013] 2) cold forming the three mixed powders to obtain green compacts A, B and C;
[0014] 3) The C green body, the B green body and the A green body are sequentially assembled from the inside to the outside to form a cemented carbide drawing die green body;
[0015] 4) Degreasing and firing the cemented carbide drawing die green body, and then using physical vapor deposition to deposit a wear-resistant layer on the inner surface of the die to obtain a high-hardness cemented carbide drawing die material.
[0016] Furthermore, in step 1), the average particle sizes of tungsten carbide powder, cobalt powder, cobalt-aluminum-tungsten high-temperature alloy powder and cobalt-nickel-molybdenum three-element alloy powder are 2-4 microns, 1-2 microns, 4-6 microns and 4-7 microns respectively.
[0017] Further, in step 1), in the mixed powder A, the tungsten carbide powder is 79% to 82%, and the cobalt powder is 18% to 21% by mass percentage;
[0018] In terms of mass percentage, in the mixed powder B, the tungsten carbide powder is 84% to 88%, and the cobalt-aluminum-tungsten high-temperature alloy powder is 12% to 16%;
[0019] In terms of mass percentage, in the mixed powder C, the tungsten carbide powder accounts for 89% to 93%, and the cobalt, nickel, and molybdenum three-element alloy powder accounts for 7% to 11%.
[0020] Furthermore, the three groups of powders were mixed using a three-dimensional vortex mixer with a main shaft speed of 140 to 170 revolutions per minute for 32 to 38 minutes.
[0021] Further, step 2) is specifically as follows:
[0022] Firstly, the three mixed powders are plasticized, and 16% to 19% by mass of PVA solution are added respectively to obtain three plasticized slurries;
[0023] The three plasticized slurries are injection molded at an injection speed of 8 to 12 ml per second, a temperature of 160 to 190° C., and a green body drying time of 15 to 21 minutes.
[0024] Furthermore, in step 4), the cemented carbide drawing die green body is subjected to a two-step treatment of degreasing and firing by gas pressure sintering, the degreasing temperature and time are 370-400° C. and 43-51 minutes, respectively, and the firing temperature and time are 1380-1415° C. and 35-42 minutes, respectively.
[0025] Further, in step 4), the wear-resistant layer is pure tungsten carbide.
[0026] Furthermore, in step 4), the physical vapor deposition method is selected from magnetron sputtering, evaporation plating or ion plating.
[0027] The present invention also discloses a high-hardness cemented carbide drawing die material prepared by the preparation method. The high-hardness cemented carbide drawing die material has a multi-layer structure, which includes, from the inside to the outside, a cobalt-nickel-molybdenum bonding phase layer, a cobalt-aluminum-tungsten high-temperature alloy bonding phase layer and a cobalt bonding phase layer.
[0028] Furthermore, the fracture toughness of the high hardness cemented carbide drawing die material is greater than or equal to 14.6 MPa·m 1 / 2 , inner surface hardness is greater than or equal to 25.3GPa, bending strength is greater than or equal to 5150MPa, and inner surface high temperature hardness is greater than or equal to 20.6GPa.
[0029] Compared with the prior art, the present invention has the following beneficial technical effects:
[0030] The invention discloses a method for preparing a high-hardness cemented carbide drawing die material. Firstly, tungsten carbide powder is respectively weighed and mixed with cobalt powder, cobalt-aluminum-tungsten high-temperature alloy powder and cobalt-nickel-molybdenum three-main alloy powder according to a certain mass percentage, and then the three-component mixed powder is cold-formed by injection molding technology, and is assembled from the inside to the outside according to the component category and shape and size requirements to form a cemented carbide drawing die green body, and then the gas pressure sintering technology is used to degrease and sinter the cemented carbide drawing die green body, and finally a wear-resistant layer is deposited on the inner surface of the die by physical vapor deposition.
[0031] Among them, the use of cobalt-nickel-molybdenum medium entropy alloy bonding phase can improve the hardness and toughness of the inner surface of the mold, and the cobalt-aluminum-tungsten high-temperature alloy bonding phase can coordinate the strength and toughness of the cobalt-nickel-molybdenum bonding phase layer and the cobalt bonding phase layer; the three bonding phases are all based on cobalt to form a multi-layer gradient structure of component content and type. Under the premise of ensuring the difference in hardness and toughness performance of the multi-layer structure, it promotes the formation of a firm interface bonding between the layers to achieve the integrity of the multi-layer gradient structure and avoid fatigue or cracking of the cemented carbide drawing die due to interlayer stress concentration under long-term service conditions; injection molding technology is used to form a hollow conical blank, providing a basis for the cold forming of the multi-layer structure. This technology is combined with the gradient component and uses the sintering principle that the larger the proportion of the bonding phase, the more conducive it is to the shrinkage of the sintered blank. It promotes the formation of a firm metallurgical bonding interface in the green body of the multi-layer cemented carbide drawing die, which is beneficial to ensure the dimensional accuracy of the mold without weakening the overall performance of the mold; the gas pressure sintering technology, on the one hand, facilitates the formation of a close metallurgical bond between the three-layer structure, and on the other hand, by increasing the sintering temperature, a liquid phase sintering mode is formed to promote sintering densification.
[0032] Furthermore, in the process of preparing cemented carbide drawing dies, the present invention aims at the engineering problem that the existing methods are difficult to simultaneously improve the inner surface hardness and overall toughness of cemented carbide drawing dies. Through multi-component collaboration, injection cold forming and multi-layer sintering series technologies, the relationship between powder components, powder mixing process parameters, injection molding process parameters, gas pressure sintering process and hardness, toughness and high-temperature mechanical properties of cemented carbide drawing dies is studied, that is: for cemented carbide drawing die materials, the best powder components, powder mixing process parameters, injection molding process parameters and gas pressure sintering process that maintain high hardness, toughness and high-temperature mechanical properties. This method has high component control accuracy, strong process stability and repeatability, and can achieve wear resistance, hardness and fatigue resistance of cemented carbide drawing dies.
[0033] The high-hardness cemented carbide drawing die material prepared by the present invention has a multi-layer structure, and the fracture toughness of the material is greater than or equal to 14.6MPa·m 1 / 2 , the inner surface hardness is greater than or equal to 25.3GPa, the bending strength is greater than or equal to 5150MPa, and the inner surface high temperature (1000℃) hardness is greater than or equal to 20.6GPa. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the following is further described in detail with reference to the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all the embodiments.
[0035] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making any creative work shall fall within the protection scope of the present invention.
[0036] The invention discloses a method for preparing a high-hardness cemented carbide drawing die material, comprising the following steps:
[0037] 1) Weighing tungsten carbide powder with an average particle size of 2 to 4 microns with cobalt powder of 1 to 2 microns, cobalt-aluminum-tungsten high-temperature alloy powder of 4 to 6 microns and cobalt-nickel-molybdenum three-main alloy powder of 4 to 7 microns in a weight percentage of 79 to 82: 18 to 21, 84 to 88: 12 to 16 and 89 to 93: 7 to 11, respectively, and mixing the three groups of powders in a three-dimensional vortex mixer at a main shaft speed of 140 to 170 revolutions per minute for 32 to 38 minutes to obtain a mixed powder of three components;
[0038] 2) Plasticizing the three groups of mixed powders, adding 16-19% PVA solution (concentration 10%) by mass respectively, injecting the plasticized slurry into the injection cavity at a speed of 8-12 ml per second, at a temperature of 160-190° C., and drying the blank for 15-21 minutes. The three-component mixed powders are cold-formed by injection molding technology, and then the three-main alloy of cobalt-nickel-molybdenum, cobalt-aluminum-tungsten high-temperature alloy powder and cobalt as the binder components are assembled from the inside to the outside, with clearance matching between layers and an error of ±0.05-0.08 mm to form a cemented carbide drawing die blank;
[0039] 3) The cemented carbide drawing die green body is subjected to two-step treatment of degreasing and firing in a gas pressure sintering device, the degreasing temperature and time are 370-400°C and 43-51 minutes respectively, and the sintering temperature and time are 1380-1415°C and 35-42 minutes respectively; the physical vapor deposition layer is pure tungsten carbide, and magnetron sputtering, evaporation plating or ion plating is selected, with a deposition thickness of 3.3-5.2 microns, and finally a high-hardness cemented carbide drawing die material is obtained.
[0040] The features and performances of the present invention are further described in detail below in conjunction with the embodiments.
[0041] Example 1
[0042] 1) In terms of mass percentage, 79% tungsten carbide powder with an average particle size of 2 μm and 21% cobalt powder with an average particle size of 1 μm were mixed to obtain mixed powder A;
[0043] In terms of mass percentage, 84% tungsten carbide powder with an average particle size of 2 microns and 16% cobalt aluminum tungsten high temperature alloy powder with a particle size of 4 microns are mixed to obtain mixed powder B;
[0044] In terms of mass percentage, 89% tungsten carbide powder with an average particle size of 2 microns and 11% cobalt-nickel-molybdenum three-main alloy powder with an average particle size of 4 microns are mixed to obtain mixed powder C;
[0045] Specifically, three groups of powders were mixed using a three-dimensional vortex mixer, with a spindle speed of 140 rpm and mixing for 32 minutes to obtain a three-component mixed powder;
[0046] 2) Plasticizing the three groups of mixed powders, adding 16% PVA solution respectively, injecting the plasticized slurry into the injection cavity at a speed of 8 ml per second, the temperature is 160° C., the blank drying time is 15 minutes, and the three-component mixed powders are cold-formed by injection molding technology, and then the three-main alloy of cobalt-nickel-molybdenum, cobalt-aluminum-tungsten high-temperature alloy powder and cobalt are assembled from the inside to the outside according to the binder components, and the gap between the layers is matched with an error of ±0.05 mm to form a cemented carbide drawing die green body;
[0047] 3) The cemented carbide drawing die green body is subjected to two-step degreasing and sintering treatment in a gas pressure sintering device. The degreasing temperature and time are 400°C and 43 minutes respectively, and the sintering temperature and time are 1380°C and 42 minutes respectively. A pure tungsten carbide layer is deposited on the inner surface of the die by vacuum evaporation plating technology with a deposition thickness of 5.2 microns, and finally a high-hardness cemented carbide drawing die material is obtained.
[0048] Example 2
[0049] 1) In terms of mass percentage, 82% tungsten carbide powder with an average particle size of 4 microns and 18% cobalt powder with an average particle size of 2 microns were mixed to obtain mixed powder A;
[0050] In terms of mass percentage, 88% tungsten carbide powder with an average particle size of 4 microns and 12% cobalt aluminum tungsten high temperature alloy powder with a particle size of 4 microns are mixed to obtain mixed powder B;
[0051] 93% tungsten carbide powder with an average particle size of 4 microns and 7% cobalt-nickel-molybdenum three-primary alloy powder with a particle size of 4 microns are mixed to obtain mixed powder C;
[0052] Among them, a three-dimensional vortex mixer was used to mix three groups of powders, with a main shaft speed of 170 rpm and mixing for 32 minutes to obtain a mixed powder of three components;
[0053] 2) Plasticizing the three groups of mixed powders, adding 10% PVA solution respectively, injecting the plasticized slurry into the injection cavity at a speed of 12 ml per second, the temperature is 190° C., the blank drying time is 21 minutes, and the three-component mixed powders are cold-formed by injection molding technology, and then the three-main alloy of cobalt, nickel, and molybdenum, the cobalt-aluminum-tungsten high-temperature alloy powder and the cobalt as the binder components are assembled from the inside to the outside, and the gap between the layers is matched with an error of ±0.08 mm to form a cemented carbide drawing die green body;
[0054] 3) The cemented carbide drawing die green body is subjected to two-step degreasing and sintering treatment in a gas pressure sintering device. The degreasing temperature and time are 400°C and 51 minutes respectively, and the sintering temperature and time are 1415°C and 35 minutes respectively. A pure tungsten carbide layer is deposited on the inner surface of the die by ion plating with a deposition thickness of 5.2 microns, and finally a high-hardness cemented carbide drawing die material is obtained.
[0055] Example 3
[0056] 1) In terms of mass percentage, 80% tungsten carbide powder with an average particle size of 3 microns and 20% cobalt powder with an average particle size of 2 microns are mixed to obtain mixed powder A;
[0057] In terms of mass percentage, 86% tungsten carbide powder with an average particle size of 3 microns and 14% cobalt aluminum tungsten high temperature alloy powder with a particle size of 5 microns are mixed to obtain mixed powder B;
[0058] 90% tungsten carbide powder with an average particle size of 3 microns and 10% cobalt-nickel-molybdenum three-principal alloy powder with an average particle size of 5 microns are mixed to obtain mixed powder C;
[0059] Among them, three groups of powders were mixed using a three-dimensional vortex mixer, with a spindle speed of 150 rpm and mixing for 35 minutes to obtain a mixed powder of three components;
[0060] 2) Plasticizing the three groups of mixed powders, adding 10% PVA solution respectively, injecting the plasticized slurry into the injection cavity at a speed of 10 ml per second, the temperature is 180° C., the blank drying time is 18 minutes, and the three-component mixed powders are cold-formed by injection molding technology, and then the three-main alloy of cobalt-nickel-molybdenum, cobalt-aluminum-tungsten high-temperature alloy powder and cobalt are assembled from the inside to the outside according to the binder components, and the gap between the layers is matched with an error of ±0.07 mm to form a cemented carbide drawing die green body;
[0061] 3) The cemented carbide drawing die green body is subjected to two-step degreasing and sintering treatment in a gas pressure sintering device. The degreasing temperature and time are 390°C and 48 minutes respectively, and the sintering temperature and time are 1395°C and 39 minutes respectively; the magnetron sputtering target is pure tungsten carbide, the RF power is preferably 310W, the deposition time is 16 minutes, and the deposition thickness is 3.9 microns, finally obtaining a high hardness cemented carbide drawing die material.
[0062] Example 4
[0063] 1) In terms of mass percentage, 81% tungsten carbide powder with an average particle size of 4 microns and 18% cobalt powder with an average particle size of 19 microns were mixed to obtain mixed powder A;
[0064] In terms of mass percentage, 87% tungsten carbide powder with an average particle size of 4 microns and 13% cobalt aluminum tungsten high temperature alloy powder with a particle size of 13 microns are mixed to obtain mixed powder B;
[0065] In terms of mass percentage, 91% tungsten carbide powder with an average particle size of 4 microns and 9% cobalt-nickel-molybdenum three-primary alloy powder with a particle size of 4 microns are mixed to obtain mixed powder C;
[0066] Among them, three groups of powders were mixed using a three-dimensional vortex mixer, with a spindle speed of 170 rpm and mixing for 37 minutes to obtain a three-component mixed powder;
[0067] 2) Plasticizing the three groups of mixed powders, adding 10% PVA solution respectively, injecting the plasticized slurry into the injection cavity at a speed of 11 ml per second, the temperature is 190° C., the blank drying time is 21 minutes, and the three-component mixed powders are cold-formed by injection molding technology, and then the three-main alloy of cobalt, nickel, and molybdenum, the cobalt-aluminum-tungsten high-temperature alloy powder and the cobalt are assembled from the inside to the outside according to the binder components, and the gap between the layers is matched with an error of ±0.07 mm to form a cemented carbide drawing die green body;
[0068] 3) The cemented carbide drawing die green body is subjected to two-step degreasing and sintering treatment in a gas pressure sintering device. The degreasing temperature and time are 380°C and 48 minutes respectively, and the sintering temperature and time are 1405°C and 39 minutes respectively; the magnetron sputtering target is pure tungsten carbide, the RF power is preferably 310W, the deposition time is 17 minutes, and the deposition thickness is 4.5 microns, finally obtaining a high-hardness cemented carbide drawing die material.
[0069] The mechanical properties of the cemented carbide drawing die materials prepared in Examples 1 to 4 were verified, and the obtained performance parameters are shown in Table 1:
[0070] Table 1
[0071]
[0072] It can be concluded from the above table that the high hardness cemented carbide drawing die material prepared by the present invention has a multilayer structure, and the fracture toughness of the material is greater than or equal to 14.6 MPa·m 1 / 2 , the inner surface hardness is greater than or equal to 25.3GPa, the bending strength is greater than or equal to 5150MPa, and the inner surface high temperature (1000℃) hardness is greater than or equal to 20.6GPa.
[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a high-hardness cemented carbide drawing die material, It is characterized in that The following steps are involved: 1) mixing tungsten carbide powder and cobalt powder to obtain mixed powder A; Tungsten carbide powder and cobalt aluminum tungsten high temperature alloy powder are mixed to obtain mixed powder B; Mixing tungsten carbide powder with cobalt, nickel and molybdenum three-element alloy powder to obtain mixed powder C; 2) cold forming the three mixed powders to obtain green compacts A, B and C; 3) The C green body, the B green body and the A green body are sequentially assembled from the inside to the outside to form a cemented carbide drawing die green body; 4) Degreasing and firing the cemented carbide drawing die green body, and then using physical vapor deposition to deposit a wear-resistant layer on the inner surface of the die to obtain a high-hardness cemented carbide drawing die material.
2. The method for preparing the high-hardness cemented carbide drawing die material according to claim 1, It is characterized in that In step 1), the average particle sizes of tungsten carbide powder, cobalt powder, cobalt-aluminum-tungsten high-temperature alloy powder and cobalt-nickel-molybdenum three-element alloy powder are 2-4 microns, 1-2 microns, 4-6 microns and 4-7 microns respectively.
3. The method for preparing the high hardness cemented carbide drawing die material according to claim 1, It is characterized in that In step 1), in the mixed powder A, the tungsten carbide powder is 79% to 82% and the cobalt powder is 18% to 21% by mass percentage; In terms of mass percentage, in the mixed powder B, the tungsten carbide powder is 84% to 88%, and the cobalt-aluminum-tungsten high-temperature alloy powder is 12% to 16%; In terms of mass percentage, in the mixed powder C, the tungsten carbide powder accounts for 89% to 93%, and the cobalt, nickel, and molybdenum three-element alloy powder accounts for 7% to 11%.
4. The method for preparing the high-hardness cemented carbide drawing die material according to claim 1, It is characterized in that The three groups of powders were mixed using a three-dimensional vortex mixer, with a main shaft speed of 140 to 170 revolutions per minute for 32 to 38 minutes.
5. The method for preparing the high-hardness cemented carbide drawing die material according to claim 1, It is characterized in that Step 2) is specifically as follows: Firstly, the three mixed powders are plasticized, and 16% to 19% by mass of PVA solution are added respectively to obtain three plasticized slurries; The three plasticized slurries are injection molded at an injection speed of 8 to 12 ml per second, a temperature of 160 to 190° C., and a green body drying time of 15 to 21 minutes.
6. The method for preparing the high-hardness cemented carbide drawing die material according to claim 1, It is characterized in that In step 4), the cemented carbide drawing die green body is subjected to a two-step treatment of degreasing and firing by gas pressure sintering, the degreasing temperature and time are 370-400° C. and 43-51 minutes, respectively, and the firing temperature and time are 1380-1415° C. and 35-42 minutes, respectively.
7. The method for preparing the high-hardness cemented carbide drawing die material according to claim 1, It is characterized in that In step 4), the wear-resistant layer is pure tungsten carbide.
8. The method for preparing the high-hardness cemented carbide drawing die material according to claim 1, It is characterized in that In step 4), the physical vapor deposition method is selected from magnetron sputtering, evaporation plating or ion plating.
9. The high-hardness cemented carbide drawing die material prepared by the preparation method according to any one of claims 1 to 8, It is characterized in that The high-hardness cemented carbide drawing die material has a multi-layer structure, which includes a cobalt-nickel-molybdenum bonding phase layer, a cobalt-aluminum-tungsten high-temperature alloy bonding phase layer and a cobalt bonding phase layer from the inside to the outside.
10. The high hardness cemented carbide drawing die material according to claim 9, It is characterized in that The fracture toughness of the high-hardness cemented carbide drawing die material is greater than or equal to 14.6 MPa·m 1 / 2 , inner surface hardness is greater than or equal to 25.3GPa, bending strength is greater than or equal to 5150MPa, and inner surface high temperature hardness is greater than or equal to 20.6GPa.