Production and manufacturing method of 2xxx / 7xxx aluminum alloy plate for aerospace

By using two spray quenching, pre-stretching and post-axial straightening treatments in the production of 2xxx/7xxx aluminum alloy plates for aerospace, the residual stress and plate shape problems in the internal plate are solved, significantly improving the elongation and plate. , quality, meet aerospace needs.

CN118979206APending Publication Date: 2024-11-19NORTHEAST LIGHT ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049667.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the machine addition process, 2xxx/7xxx aluminum alloy plates for aerospace are prone to cracking due to large internal residual stress and excessive unevenness. The prior art is difficult to effectively eliminate residual stress and improve the plate type.

Method used

Two spray quenching, pre-stretching and aging treatment methods are adopted to improve the uniformity of the residual phases inside the tissue through the second quenching, increase the stretching amount to reduce residual stress, and straighten the treatment after aging to improve the plate type.

Benefits of technology

It significantly improves the elongation of the plate, eliminates internal residual stress, improves the plate shape, meets the use needs of 2xxx/7xxx aluminum alloy plates for aerospace, and avoids cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979206A_ABST
    Figure CN118979206A_ABST
Patent Text Reader

Abstract

The invention discloses a production and manufacturing method of a 2xxx / 7xxx aluminum alloy plate for aerospace, and aims to solve the problem that the existing 2xxx / 7xxx aluminum alloy plate for aerospace often cracks in a machining process due to large internal residual stress, out-of-tolerance unevenness and the like in the machining process of the plate. The 2xxx / 7xxx aluminum alloy plate for aerospace is subjected to primary quenching, and the aluminum alloy plate subjected to primary quenching is subjected to secondary quenching, pre-stretching, aging treatment and straightening treatment to form an aluminum alloy plate finished product. On the basis of an existing process, the straightening process and the secondary quenching process are added, the uniformity of a structure residual phase can be improved through secondary quenching, the ductility of the plate is improved, the residual stress in the structure can be better reduced through the subsequent large stretching amount, and the use requirement of the 2xxx / 7xxx aluminum alloy plate is better met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a 2xxx / 7xxx aluminum alloy sheet for aerospace Background Art

[0002] With the rapid development of my country's aerospace industry, more stringent requirements have been put forward for basic materials. For 2xxx / 7xxx aluminum alloy plates used in aerospace, the plates often crack during the machining process due to large internal residual stress and excessive unevenness. Therefore, eliminating the residual stress of the plate structure and improving the plate shape are the top priorities for solving the problem of heat-treatable and strengthened 2xxx / 7xxx aluminum alloy plates. Summary of the invention

[0003] The present invention aims to maintain the performance of 2xxx / 7xxx aluminum alloy plates for aerospace use, improve the elongation while reducing the internal residual stress by changing the structure of the plates after quenching, and finally improve the plate shape of the finished plates through straightening treatment, thereby meeting the use requirements of 2xxx / 7xxx aluminum alloy plates for aerospace use.

[0004] The manufacturing method of the 2xxx / 7xxx aluminum alloy sheet for aerospace of the present invention provides the following technical solutions:

[0005] (1) First quenching: heating the aluminum alloy plate, heating and keeping the aluminum alloy plate warm for a certain period of time, taking the aluminum alloy plate out of the heating furnace, and then immediately quenching the aluminum alloy plate by spraying;

[0006] (2) Second quenching: The aluminum alloy plate that has been quenched for the first time is reheated. After heating and keeping warm for a certain period of time, the aluminum alloy plate is taken out of the heating furnace, and then the aluminum alloy plate is immediately quenched for the second time by spraying;

[0007] (3) Stretching: Pre-stretching the aluminum alloy sheet by 2.5-2.7% using a stretching machine;

[0008] (4) Aging: The aluminum alloy sheet is kept warm for a set time;

[0009] (5) Straightening: The aluminum alloy sheet is sawn and straightened to form a finished aluminum alloy sheet.

[0010] Preferably, in the above-mentioned method for producing the aluminum alloy plate, the heating and insulation time of the aluminum alloy plate in step (2) is performed according to the first quenching process.

[0011] Preferably, in the above-mentioned method for producing the aluminum alloy sheet, the pre-stretching deformation of the aluminum alloy sheet in step (3) is 2.6%.

[0012] Preferably, in the above-mentioned method for producing the aluminum alloy sheet, the straightening temperature of the aluminum alloy sheet in step (5) is room temperature.

[0013] The manufacturing method of the 2xxx / 7xxx aluminum alloy plate for aerospace provided by the present invention performs a second quenching on the basis of the existing production process. The second quenching makes the residual phase inside the organization more fine and uniform, so that the elongation is greatly improved. When the elongation is significantly improved, the stretching amount is increased to eliminate the internal residual stress. At the same time, the plate is straightened after aging to improve the plate shape, thereby meeting the use requirements of the 2xxx / 7xxx aluminum alloy plate for aerospace. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. It is obvious that the drawings described below are only part of the embodiments of the present invention. Other technicians in this field can also obtain other drawings based on these drawings.

[0015] Figure 1 A schematic diagram of the organization of the embodiment 1 of the production method of the 2xxx / 7xxx aluminum alloy plate provided by the embodiment of the present invention; wherein the left figure is a schematic diagram of the organization of the core of the plate after a single quenching, and the right figure is a schematic diagram of the organization of the edge of the plate after a single quenching;

[0016] Figure 2 The schematic diagram of the organization of Example 2 of the production and manufacturing method of 2xxx / 7xxx aluminum alloy plate provided in the embodiment of the present invention; wherein the left figure is a schematic diagram of the core organization of the plate after the second quenching, and the right figure is a schematic diagram of the edge organization of the plate after the second quenching. DETAILED DESCRIPTION

[0017] Embodiment 1:

[0018] Please refer to the attached Figure 1 , Figure 1 This is a schematic diagram of the organization of the first embodiment of the production method of the 2xxx / 7xxx aluminum alloy plate; the specific method is as follows:

[0019] Primary quenching: heating the aluminum alloy plate, heating and keeping the aluminum alloy plate warm for a certain period of time, taking the aluminum alloy plate out of the heating furnace, and then immediately quenching the aluminum alloy plate by spraying to improve the performance of the plate;

[0020] Stretching: using a stretching machine to pre-stretch the aluminum alloy sheet with a stretching amount of 1.7-2.0% to reduce the residual stress inside the sheet;

[0021] Aging: The aluminum alloy sheet is kept warm for a set time to improve the performance of the sheet through aging strengthening;

[0022] Straightening: After aging, the plate is straightened. Straightening can further eliminate the residual stress inside the plate. Most importantly, it can improve the plate shape and ensure that the plate does not crack during the machining process.

[0023] The production and manufacturing method of the 2xxx / 7xxx aluminum alloy plate provided by the present invention adds a straightening treatment after the aging process on the basis of the existing process. After straightening, the residual stress inside the structure is reduced, and the plate shape is further improved, and the machining deformation is reduced. At the same time, the unevenness of the plate after the straightening treatment meets the user's usage requirements.

[0024] Embodiment 2:

[0025] Please refer to the attached Figure 2 , Figure 2 This is a schematic diagram of the organization of the second embodiment of the production method of the 2xxx / 7xxx aluminum alloy plate. The specific method is as follows:

[0026] First quenching: heating the aluminum alloy plate, heating and keeping the aluminum alloy plate warm for a certain period of time, taking the aluminum alloy plate out of the heating furnace, and then immediately quenching the aluminum alloy plate by spraying to improve the performance of the plate;

[0027] Second quenching: The aluminum alloy plate that has been quenched for the first time is reheated. After heating and keeping warm for a certain period of time, the aluminum alloy plate is taken out of the heating furnace, and then immediately quenched for the second time by spraying. Through the second quenching, the uniformity of the residual phase of the structure is improved and the elongation of the plate is increased.

[0028] Stretching: using a stretching machine to pre-stretch the aluminum alloy sheet, the stretching amount is 2.5-2.7%, and the residual stress inside the sheet is reduced by increasing the stretching amount;

[0029] Aging: The aluminum alloy sheet is kept warm for a set time to improve the performance of the sheet through aging strengthening;

[0030] Straightening: After aging, the plate is straightened. Straightening can further eliminate the residual stress inside the plate. Most importantly, it can improve the plate shape and ensure that the plate does not crack during the machining process.

[0031] In the above embodiments, the second quenching is mainly used. By performing a second quenching on the plate after the first quenching, the tensile strength and the yield strength are basically unchanged, but the elongation will be greatly improved, which is more conducive to the use requirements of 2xxx / 7xxx aluminum alloy plates.

[0032] In the above embodiments, the stretching amount is mainly increased. The greater the stretching amount, the greater the reduction in residual stress inside the tissue. Since the secondary quenching has been performed, the better the toughness is, the more suitable it is for a larger stretching amount to be used, thereby reducing internal residual stress.

Claims

1. A method for producing 2xxx / 7xxx aluminum alloy sheets for aerospace, characterized in that It is carried out according to the following steps: (1) First quenching: heating the aluminum alloy plate, after the aluminum alloy plate is heated and kept warm, taking the aluminum alloy plate out of the heating furnace, and then immediately quenching the aluminum alloy plate by spraying; (2) Second quenching: reheating the aluminum alloy plate that has been quenched for the first time, taking the aluminum alloy plate out of the heating furnace after heating and heat preservation, and then immediately quenching the aluminum alloy plate for the second time by spraying; (3) Stretching: Pre-stretching the aluminum alloy sheet by 2.5-2.7% using a stretching machine; (4) Aging: The stretched aluminum alloy sheet is kept warm for a set time; (5) Straightening: The aluminum alloy sheet after sawing and insulation is straightened to form a finished aluminum alloy sheet.

2. The method for producing a 2xxx / 7xxx aluminum alloy sheet for aerospace according to claim 1, characterized in that The first quenching heating temperature described in step (1) is 470° C. to 498° C., and the holding time is 130 min to 160 min.

3. The method for producing a 2xxx / 7xxx aluminum alloy sheet for aerospace according to claim 1, characterized in that The second quenching heating temperature described in step (2) is 470° C. to 498° C., and the holding time is 95 min to 130 min.

4. The method for producing a 2xxx / 7xxx aluminum alloy sheet for aerospace according to claim 1, characterized in that The stretching amount in step (3) is 2.6%.

5. The method for producing a 2xxx / 7xxx aluminum alloy sheet for aerospace according to claim 1, characterized in that The straightening temperature of the aluminum alloy plate described in step (5) is room temperature.