Novel iron-based amorphous alloy coating hole sealing agent and hole sealing process thereof

Through the hybrid sealing treatment of inorganic-organic composite pore sealing agent, the corrosion problem caused by pore defects of the iron-based amorphous coating is solved, and efficient sealing, superhydrophobicity and self-cleaning are achieved. It is suitable for large parts and structural engineering parts. Reduces cost and operational complexity.

CN118979218AActive Publication Date: 2024-11-19INST OF METAL RESEARCH - CHINESE ACAD OF SCI +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411076157.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing iron-based amorphous coatings are prone to pore defects during spraying, resulting in corrosion problems. The traditional pore sealing process is costly and complex, making it difficult to be suitable for large components and structural engineering components.

Method used

Using hybrid sealing treatment of inorganic-organic composite sealing agent, a neodymium-based rare earth oxide film is formed through inorganic rare earth sealing agent, and surface modification and sealing is combined with organic sealing agent to achieve efficient sealing, superhydrophobicity of the coating and Self-cleaning.

Benefits of technology

It significantly improves the sealing and corrosion resistance of the coating, reduces the cost of sealing holes, simplifies the process flow, gives the coating superhydrophobicity and self-cleaning, and is suitable for large parts and structural engineering parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979218A_ABST
    Figure CN118979218A_ABST
Patent Text Reader

Abstract

The invention discloses a novel iron-based amorphous alloy coating hole sealing agent and a hole sealing process thereof, and relates to the technical field of surface engineering, the hole sealing agent is a combination of an inorganic rare earth hole sealing agent and an organic hole sealing machine, and a preparation method of the hole sealing agent comprises the following steps: S1, coating surface treatment; s2, preparing an inorganic sealant; s3, preparing an organic sealant; s4, hole sealing treatment is conducted on the coating; the method has the following advantages: (1) the novel hole sealing agent is non-toxic, safe and green; (2) the hole sealing process is simple, and complex steps such as heating hole sealing, vacuum hole sealing or ultrasonic hole sealing required by a traditional hole sealing agent are avoided; and (3) the corrosion resistance of the coating after hole sealing is greatly improved, the surface of the coating is endowed with super-hydrophobicity and self-cleaning property, and the antifouling property of the surface of the coating is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface engineering, in particular to a pore sealing method for an iron-based amorphous coating. Background Art

[0002] The iron-based amorphous alloy coating produced by supersonic flame spraying technology has excellent corrosion resistance due to its low crystal defects and long-term disorder, which greatly improves its application in industries such as nuclear waste storage facilities and offshore anti-corrosion components. However, due to the shielding effect caused by different spraying angles, particle rebound and coating shrinkage during solidification during the spraying process, serious pore defects will inevitably be generated in the coating. As liquid channels, the pores will promote the penetration of electrolytes into the coating / substrate interface. This will cause the coating to delaminate and eventually peel off. Porosity-induced corrosion is one of the most common failure modes of engineering structures. Sealing treatment technology is widely used in the sealing of porous coatings due to its simple operation and low manufacturing cost. The pores on the surface and inside of the coating are infiltrated, blocked and filled by the sealant to improve the density of the coating and inhibit the migration of corrosion factors.

[0003] Most of the currently used sealing processes for amorphous coatings are performed by heating the sealing agent or combining special treatments, such as electrochemical polarization treatment, vacuum infiltration and ultrasonic assistance, but too high a temperature will cause the amorphous coating to crystallize, which will change the intrinsic excellent performance of the coating. Special treatment is acceptable for small components, but for special large components and actual structural engineering components, in addition to complicated operations, the cost will also be greatly increased. Therefore, the sealing method of an iron-based amorphous coating of the present invention can effectively solve the above problems, and has low cost, simple operation, and greatly improved corrosion performance. Summary of the invention

[0004] In order to solve the problem of pore-induced corrosion of key components of iron-based amorphous coating equipment, the iron-based amorphous coating is further sealed. The present invention provides a pore sealing method for iron-based amorphous coating, which not only achieves efficient sealing of the coating, but also realizes excellent super-hydrophobicity and self-cleaning properties, and takes into account outstanding corrosion resistance. It has the advantages of simple surface treatment process, high efficiency and low cost.

[0005] To achieve the above object, the technical solution adopted by the present invention is as follows: a sealing method for an iron-based amorphous coating, comprising the following steps:

[0006] (1) Coating surface treatment: Clean the coating surface to be treated;

[0007] (2) Preparation of inorganic sealant: Disperse 5-10 g (preferably 5-8 g) of neodymium nitrate and 10-15 ml (preferably 10-12 ml) of hydrogen peroxide (mass concentration 10-30%) into 500 ml of deionized water, and stir to obtain an inorganic sealant;

[0008] (3) Preparation of organic sealant: butyl acetate is added to epoxy resin for dilution to obtain a mixed solution, wherein the amount of butyl acetate added is 75% to 95% of the mass of the mixed solution; then 1H,1H,2H,2H-perfluorodecyltriethylsilane (FDTES) is added to the mixed solution for surface modification, wherein the amount of FDTES added is 1% to 3% of the mass of the organic sealant, and finally an organic sealant is obtained;

[0009] (4) Sealing the coating: The sealing method is an immersion method, in which the coating is first immersed in an inorganic rare earth sealing agent, and then immersed in an organic sealing agent after drying, and then dried and solidified to obtain a sealed coating.

[0010] Preferably, the iron-based amorphous coating is prepared by performing multiple sprayings on the surface of the pretreated substrate using the high velocity flame spraying (HVAF) technology to prepare an iron-based amorphous coating with a micron-level roughness; the iron-based amorphous alloy composition is: Fe 余量 Cr 18-21 Mo 5-9 Ni 2-5 P 9-15 B 1-5 C 2-6 Si 1-5 (at.% atomic percentage).

[0011] The HVAF supersonic flame spraying process is to heat and melt the iron-based amorphous alloy powder with a particle size range of 18 to 53 μm and spray it onto the surface of the substrate or component;

[0012] The HVAF supersonic flame spraying process parameters are: air pressure 70-90psi (preferably 75-85psi); propane gas pressure 70-95psi (preferably 75-90psi); propane flow rate: 90-160SLPM (110-150SLPM); hydrogen flow rate: 10-40SLPM (20-30SLPM); nitrogen flow rate: 10-30SLPM (15-25SLPM); powder feeding rate: 40-70g / min (preferably 45-65g / min); spraying distance: 200-350mm (preferably 220-300mm);

[0013] The coating thickness obtained was between 400-500 μm.

[0014] Preferably, the cleaning process in step (1) is: cleaning the coating with acetone solution and deionized water in sequence, and finally cleaning the coating with ethanol, and then drying it naturally for more than 5 minutes, preferably 10-30 minutes.

[0015] Preferably, the stirring time in step (2) is more than 5 min, preferably 20-40 min.

[0016] Preferably, the epoxy resin in step (3) is bisphenol A epoxy resin.

[0017] Preferably, the sealing method in step (4) is an immersion method:

[0018] First, immerse the surface-treated coating into an inorganic rare earth sealing agent for 10 to 50 minutes (preferably 15 to 45 minutes, more preferably 20 to 40 minutes) to allow the inorganic sealing agent to penetrate into the pores of the coating and form a neodymium-based rare earth conversion film on the coating surface. Remove the coating and dry it in air at room temperature for 1 to 6 hours (preferably 2 to 5 hours, more preferably 2 to 4 hours).

[0019] Secondly, after inorganic sealing, the coating is immersed in an organic sealing agent for organic sealing and surface modification. The immersion time is 20 to 100 minutes (preferably 40-80 minutes, more preferably 50-70 minutes), and finally a drying and curing treatment is performed; the drying and curing treatment process is room temperature drying for 8-24 hours (preferably 10-16 hours, more preferably 12-14 hours), and finally a sealing coating is obtained.

[0020] The principle of the method described in the present invention is: by carrying out hybrid sealing treatment of inorganic-organic composite sealing agent on iron-based amorphous alloy coating, the sealing property of iron-based amorphous coating is improved, and the coating is also given higher corrosion resistance and self-cleaning property. The main principle is to form a neodymium-based rare earth oxide film on the surface of the coating while using inorganic rare earth sealing agent to seal the iron-based amorphous coating for the first time. This rare earth oxide conversion film not only has a good shielding effect, but also has a large number of hydroxyl groups on the surface, which is convenient for the grafting and surface modification of organic sealing agent. The organic sealing machine realizes the second sealing of the coating. In addition to filling the cracks on the surface of the coating after the inorganic rare earth sealing agent, the bonding strength between the sealing agent and the coating is further enhanced, and the coating is given a new function, realizing super-hydrophobicity. Therefore, the corrosion resistance of the coating can be significantly improved by using the inorganic-organic composite synergistic sealing effect.

[0021] The beneficial effects of the present invention are:

[0022] (1) The new sealing agent of the invention is non-toxic, safe and green;

[0023] (2) The sealing process is simple, avoiding the complex steps of heating, vacuum sealing or ultrasonic sealing required by traditional sealing agents;

[0024] (3) After sealing, the corrosion resistance of the coating is greatly improved, and the coating surface is endowed with superhydrophobicity and self-cleaning properties, thereby improving the antifouling performance of the coating surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The iron-based amorphous coating prepared in the present invention: (a) is the DSC graph of the coating, (b) is the XRD graph of the coating, and (c) is the TEM graph of the coating;

[0026] Figure 2 is a flow chart of the preparation of the sealant of the present invention;

[0027] Figure 3 (a) and (c) are surface and cross-sectional SEM images of the original coating of the present invention; (b) and (d) are surface and cross-sectional SEM images of the sealing coating of the present invention;

[0028] Figure 4 The water jet test of the coating after sealing of the present invention;

[0029] Figure 5 The electrochemical results of the coating after sealing of the present invention;

[0030] Figure 6 is the wetting behavior of Comparative Examples 1 and 2;

[0031] Figure 7 The electrochemical results of Comparative Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with the accompanying drawings and Examples. The following examples are intended to facilitate understanding of the present invention without any limiting effect thereon. Without departing from the spirit and substance of the present invention, modifications and replacements made to the inventive method, steps or conditions all belong to the scope of the present invention. If not otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.

[0033] Example 1

[0034] A sealing method for an iron-based amorphous coating comprises the following steps:

[0035] The iron-based amorphous coating is prepared by multi-pass spraying on the surface of the pretreated substrate using the supersonic flame spraying (HVAF) technology to prepare an iron-based amorphous coating with micron-level roughness; the iron-based amorphous alloy composition is: Fe 50 Cr 18 Mo 7.5 Ni 3.5 P 12 B 3 C 3.5 Si 2.5 (at.% atomic ratio).

[0036] The HVAF supersonic flame spraying process is to heat and melt the iron-based amorphous alloy powder with a particle size range of 35μm and spray it onto the substrate or component surface;

[0037] The HVAF supersonic flame spraying process parameters are: air pressure 80psi; propane gas pressure 80psi; propane flow rate: 130SLPM; hydrogen flow rate: 25SLPM; nitrogen flow rate: 23SLPM; powder feeding rate: 60g / min; spraying distance: 260mm;

[0038] The coating thickness obtained was 450 μm.

[0039] (1) Coating surface treatment: The coating surface to be treated is cleaned; the cleaning process is: the coating is cleaned with acetone solution and deionized water in sequence, and finally the coating is cleaned with ethanol, and then naturally dried for 15 minutes.

[0040] (2) Preparation of inorganic sealant: 5 g of neodymium nitrate and 10 ml of hydrogen peroxide (mass concentration 20%) were dispersed in 500 ml of deionized water and stirred for 30 min to obtain an inorganic sealant;

[0041] (3) Preparation of organic sealant: butyl acetate is added to bisphenol A epoxy resin for dilution to obtain a mixed solution, wherein the amount of butyl acetate added is 85% of the mass of the mixed solution; then 1H,1H,2H,2H-perfluorodecyltriethylsilane (FDTES) is added to the mixed solution for surface modification, wherein the amount of FDTES added is 1% of the mass of the organic sealant, and finally an organic sealant is obtained;

[0042] (4) Sealing the coating: The sealing method is the immersion method. First, the surface-treated coating is immersed in an inorganic rare earth sealing agent for 35 minutes to allow the inorganic sealing agent to penetrate into the pores of the coating and form a neodymium-based rare earth conversion film on the surface of the coating. The coating is removed and dried in air at room temperature for 2 hours.

[0043] Secondly, after inorganic sealing, the coating is immersed in an organic sealing agent for organic sealing and surface modification. The immersion time is 50 minutes, and finally a drying and curing treatment is performed. The drying and curing process is room temperature drying for 12 hours to finally obtain a sealing coating.

[0044] Result analysis: Figure 1(a) and (b) are the DSC spectrum and XRD spectrum of the iron-based amorphous coating under Example 1. In order to quantify the amorphous content in the iron-based amorphous layer, the DSC heat flow diagrams of the strip and coating samples are given. The amorphous phase fraction contained in the coating can be evaluated by the crystallization enthalpy (ΔH), that is, in the DSC curve, the ratio of the crystallization enthalpy ΔH of the coating and the strip sample. The amorphous content of the coating is calculated to be 98.9%, which is almost completely amorphous. In the XRD spectrum of the iron-based amorphous coating and the strip, there is a wide diffuse diffraction peak between 2θ=40°-50°, and the position and shape of the XRD spectrum peaks of the coating and the strip are highly consistent, showing typical amorphous characteristics. Figure 1 (c) is the TEM image of the iron-based amorphous coating. The disordered arrangement of atoms in the high-resolution TEM image and the diffuse halo in the selected area diffraction electron map (SAED) indicate that the amorphous coating after spraying presents a completely amorphous structure.

[0045] Figure 2 The flow chart of the preparation of the sealant under Example 1 is as follows: first, an inorganic sealant is prepared, and then the coating is immersed in the inorganic sealant so that the inorganic sealant penetrates into the pores of the coating. After 35 minutes, the coating is taken out and dried at room temperature for 2 hours to obtain an inorganic sealing coating. Secondly, an organic sealant is prepared, and the coating is immersed in the organic sealant for organic sealing and surface modification. The immersion time is 50 minutes, and finally a drying and curing treatment is performed. The drying and curing process is drying at room temperature for 12 hours.

[0046] Figure 3 These are the SEM results of the untreated original coating and the sealing coating in Example 1. Figure 3 (a) and (c) are the surface and cross-sectional SEM images of the untreated original coating, respectively. Figure 3 (b) and (d) are the surface and cross-sectional SEM images of the coating after sealing, respectively. The results show that the untreated original coating presents a rough and uneven surface and cross-section. The reason for this rough surface is that the molten particles splash and rebound during the spraying process, so the original coating surface presents an uneven rough structure. After sealing, the coating surface is smooth and flat, and the neodymium oxide produced by the inorganic sealing is deposited in the pore position. At the same time, the organic resin can further seal the coating surface. The cross-sectional morphology also indirectly verifies this result. After the sealing treatment, it can be found that the coating cross-section becomes smoother. The SEM results show that the sealing plays a significant filling role.

[0047] Figure 4 This is a water jet test of the coating after sealing under Example 1. The surface of the coating is covered with hydrophilic nanopowder pollutants. During the jet test, the pollutants on the surface of the coating roll down with the water flow, showing good anti-fouling properties. The contact angle of the coating after sealing is 156°, showing super hydrophobicity.

[0048] Figure 5 This is the electrochemical polarization curve of the sealed coating in Example 1. The test environment is a 3.5% mass concentration NaCl solution. It can be found that compared with the original coating, the self-corrosion potential of the sealed iron-based amorphous coating is increased while the self-corrosion current density is reduced by nearly three orders of magnitude, which shows that the sealing treatment can effectively improve the corrosion resistance of the coating.

[0049] Example 2

[0050] A sealing method for an iron-based amorphous coating comprises the following steps:

[0051] The iron-based amorphous coating is prepared by multi-pass spraying on the surface of the pretreated substrate using the supersonic flame spraying (HVAF) technology to prepare an iron-based amorphous coating with micron-level roughness; the iron-based amorphous alloy composition is: Fe 50 Cr 18 Mo 7. 5 Ni 3.5 P 12 B 3 C 3.5 Si 2.5 (at.% atomic ratio).

[0052] The HVAF supersonic flame spraying process is to heat and melt the iron-based amorphous alloy powder with a particle size range of 40μm and spray it onto the substrate or component surface;

[0053] The HVAF supersonic flame spraying process parameters are: air pressure 75psi; propane gas pressure 70psi; propane flow rate: 125SLPM; hydrogen flow rate: 30SLPM; nitrogen flow rate: 30SLPM; powder feeding rate: 50g / min; spraying distance: 300mm;

[0054] The coating thickness obtained was 400 μm.

[0055] (1) Coating surface treatment: The coating surface to be treated is cleaned; the cleaning process is: the coating is cleaned with acetone solution and deionized water in sequence, and finally the coating is cleaned with ethanol, and then naturally dried for 20 minutes.

[0056] (2) Preparation of inorganic sealant: 8 g of neodymium nitrate and 12 ml of hydrogen peroxide (mass concentration 30%) were dispersed in 500 ml of deionized water and stirred for 35 min to obtain an inorganic sealant;

[0057] (3) Preparation of organic sealant: butyl acetate is added to bisphenol A epoxy resin for dilution to obtain a mixed solution, wherein the amount of butyl acetate added is 90% of the mass of the mixed solution; then 1H,1H,2H,2H-perfluorodecyltriethylsilane (FDTES) is added to the mixed solution for surface modification, wherein the amount of FDTES added is 2% of the mass of the organic sealant, and finally an organic sealant is obtained;

[0058] (4) Sealing the coating: The sealing method is an immersion method. First, the surface-treated coating is immersed in an inorganic rare earth sealing agent for 40 minutes to allow the inorganic sealing agent to penetrate into the pores of the coating and form a neodymium-based rare earth conversion film on the surface of the coating. The coating is then removed and dried in air at room temperature for 3 hours.

[0059] Secondly, after inorganic sealing, the coating is immersed in an organic sealing agent for organic sealing and surface modification. The immersion time is 60 minutes, and finally a drying and curing treatment is performed. The drying and curing process is room temperature drying for 13 hours to finally obtain a sealing coating.

[0060] Result analysis: In the DSC curve of Example 2, the ratio of the crystallization enthalpy ΔH of the coating and the strip sample is used to calculate the amorphous content of the coating to be 99.2%, which is almost completely amorphous. Through XRD analysis, the position and shape of the XRD peaks of the coating and the strip are highly consistent, showing typical amorphous characteristics. The TEM results of the coating are consistent with those of Example 1.

[0061] The preparation flow chart of the sealant in Example 2 is the same as that in Example 1. The difference is that in the preparation of the inorganic sealant, the coating is immersed in the inorganic sealant for 40 minutes and the room temperature drying time is 3 hours. In the preparation of the organic sealant, the coating is immersed in the organic sealant for 60 minutes and the final drying and curing time is 13 hours.

[0062] The SEM results of the untreated original coating and the sealing coating in Example 2 are consistent with those in Example 1.

[0063] The sealed coating in Example 2 was analyzed by a water jet experiment, and the results also showed good self-cleaning properties, and the contact angle of the sealed coating was as high as 158°, showing super hydrophobicity.

[0064] Electrochemical polarization curve of the sealed coating in Example 2. The test environment is also 3.5% NaCl solution, and the self-corrosion current density of the sealed iron-based amorphous coating is also reduced by nearly three orders of magnitude, indicating that the sealing treatment can effectively improve the corrosion resistance of the coating.

[0065] Comparative Example 1

[0066] In order to prove the inventiveness of the invention, we carried out a single inorganic sealing process, including the following steps:

[0067] The iron-based amorphous coating is prepared by multi-pass spraying on the surface of the pretreated substrate using the supersonic flame spraying (HVAF) technology to prepare an iron-based amorphous coating with micron-level roughness; the iron-based amorphous alloy composition is: Fe 50 Cr 18 Mo 7. 5 Ni 3.5 P 12 B 3 C 3.5 Si 2.5 (at.% atomic ratio).

[0068] The HVAF supersonic flame spraying process is to heat and melt the iron-based amorphous alloy powder with a particle size range of 45μm and spray it onto the substrate or component surface;

[0069] The HVAF supersonic flame spraying process parameters are: air pressure 80psi; propane gas pressure 80psi; propane flow rate: 130SLPM; hydrogen flow rate: 25SLPM; nitrogen flow rate: 23SLPM; powder feeding rate: 60g / min; spraying distance: 260mm;

[0070] The coating thickness obtained was 400 μm.

[0071] (1) Coating surface treatment: The coating surface to be treated is cleaned; the cleaning process is: the coating is cleaned with acetone solution and deionized water in sequence, and finally the coating is cleaned with ethanol, and then naturally dried for 20 minutes.

[0072] (2) Preparation of inorganic sealant: 5 g of neodymium nitrate and 10 ml of hydrogen peroxide (mass concentration 20%) were dispersed in 500 ml of deionized water and stirred for 35 min to obtain an inorganic sealant;

[0073] (3) immersing the surface-treated coating into an inorganic rare earth sealing agent for 40 minutes, allowing the inorganic sealing agent to penetrate into the pores of the coating and form a neodymium-based rare earth conversion film on the surface of the coating, removing the coating and drying it in air at room temperature for 3 hours to finally obtain a single inorganic sealing coating;

[0074] Results analysis: In comparative example 1, the contact angle of the coating after a single inorganic seal is as follows Figure 6As shown in the figure, after a single inorganic seal, the contact angle results all show hydrophilic behavior (water contact angle is less than 90°), mainly because a large amount of neodymium oxide is deposited on the coating surface after the inorganic seal, and the oxidized surface is rich in a large number of hydroxyl groups. A single inorganic seal does not achieve super-hydrophobic behavior. The self-cleaning performance does not reach the effect of Examples 1 and 2.

[0075] In comparative example 1, the electrochemical results of the single inorganic sealing coating are as follows: Figure 7 As shown in the polarization curve results, although the corrosion resistance of the coating is improved after single inorganic sealing, it is only improved by nearly one order of magnitude, and the performance still cannot reach the effect of Examples 1 and 2.

[0076] Comparative Example 2

[0077] In order to prove the inventiveness of the claims of the present invention, we conducted a single organic sealing process, including the following steps:

[0078] The iron-based amorphous coating is prepared by multi-pass spraying on the surface of the pretreated substrate using the supersonic flame spraying (HVAF) technology to prepare an iron-based amorphous coating with micron-level roughness; the iron-based amorphous alloy composition is: Fe 50 Cr 18 Mo 7. 5 Ni 3.5 P 12 B 3 C 3.5 Si 2.5 (at.% atomic ratio).

[0079] The HVAF supersonic flame spraying process is to heat and melt the iron-based amorphous alloy powder with a particle size range of 45μm and spray it onto the substrate or component surface;

[0080] The HVAF supersonic flame spraying process parameters are: air pressure 80psi; propane gas pressure 80psi; propane flow rate: 130SLPM; hydrogen flow rate: 25SLPM; nitrogen flow rate: 23SLPM; powder feeding rate: 60g / min; spraying distance: 260mm;

[0081] The coating thickness obtained was 400 μm.

[0082] (1) Coating surface treatment: The coating surface to be treated is cleaned; the cleaning process is: the coating is cleaned with acetone solution and deionized water in sequence, and finally the coating is cleaned with ethanol, and then naturally dried for 20 minutes.

[0083] (2) adding butyl acetate to bisphenol A epoxy resin for dilution to obtain a mixed solution, wherein the amount of butyl acetate added is 90% of the mass of the mixed solution; then adding 1H,1H,2H,2H-perfluorodecyltriethylsilane (FDTES) to the mixed solution for surface modification, wherein the amount of FDTES added is 2% of the mass of the organic sealing agent, and finally obtaining an organic sealing agent;

[0084] (3) Immersing the coating into an organic sealing agent for organic sealing and surface modification, the immersion time is 60 minutes, and finally drying and curing treatment is performed; the drying and curing process is room temperature drying for 13 hours, and finally a single organic sealing coating is obtained.

[0085] Results analysis: In comparative example 2, the contact angle of the coating after a single organic seal is as follows Figure 6 As shown, after a single organic seal, the contact angle results show hydrophobic behavior (water contact angle is between 90° and 150°), and a single organic seal does not achieve super hydrophobic behavior. The self-cleaning performance does not reach the effect of Examples 1 and 2.

[0086] In comparative example 1, the electrochemical results of the single organic sealing coating are as follows: Figure 7 As shown in the polarization curve results, although the corrosion resistance of the coating after single organic sealing is improved, it is only improved by nearly one order of magnitude, and the performance still cannot reach the effect of Examples 1 and 2.

Claims

1. A novel iron-based amorphous alloy coating sealing process, characterized in that: The method comprises the following steps: (1) Coating surface treatment: Clean the coating surface to be treated; (2) Preparation of inorganic sealant: Disperse 5-10 g (preferably 5-8 g) of neodymium nitrate and 10-15 ml (preferably 10-12 ml) of hydrogen peroxide (mass concentration 10-30%) in 500 ml of deionized water. Stirring to obtain an inorganic sealing agent; (3) Preparation of organic sealant: butyl acetate is added to epoxy resin for dilution to obtain a mixed solution, wherein the amount of butyl acetate added is 75% to 95% of the mass of the mixed solution; then 1H,1H,2H,2H-perfluorodecyltriethylsilane (FDTES) is added to the mixed solution for surface modification, wherein the amount of FDTES added is 1% to 3% of the mass of the organic sealant, and finally an organic sealant is obtained; (4) Sealing the coating: The sealing method is an immersion method, in which the coating is first immersed in an inorganic rare earth sealing agent, and then immersed in an organic sealing agent after drying, and then dried and cured to obtain a sealed coating.

2. The sealing process according to claim 1, characterized in that: The iron-based amorphous coating is prepared by spraying multiple times on the surface of the pretreated substrate using the high velocity flame spraying (HVAF) technology to prepare an iron-based amorphous coating with a micron-level roughness; the iron-based amorphous alloy composition is: Fe 余量 Cr 18-21 Mo 5-9 Ni 2-5 P 9-15 B 1-5 C 2-6 Si 1-5 (at.% atomic percentage); The HVAF supersonic flame spraying process is to heat and melt the iron-based amorphous alloy powder with a particle size range of 18 to 53 μm and spray it onto the surface of the substrate or component; The HVAF supersonic flame spraying process parameters are: air pressure 70-90psi (preferably 75-85psi); propane gas pressure 70-95psi (preferably 75-90psi); propane flow rate: 90-160SLPM (110-150SLPM); hydrogen flow rate: 10-40SLPM (20-30SLPM); nitrogen flow rate: 10-30SLPM (15-25SLPM); powder feeding rate: 40-70g / min (preferably 45-65g / min); spraying distance: 200-350mm (preferably 220-300mm); The coating thickness obtained was between 400-500 μm.

3. The sealing process according to claim 1, characterized in that: In step (1), the cleaning process is: the coating is cleaned with acetone solution and deionized water in sequence, and finally the coating is cleaned with ethanol, and then naturally dried for more than 5 minutes, preferably 10-30 minutes.

4. The sealing process according to claim 1, characterized in that: In step (2), the stirring time is more than 5 min, preferably 20-40 min.

5. The sealing process according to claim 1, characterized in that: In step (3), the epoxy resin is bisphenol A epoxy resin.

6. The sealing process according to claim 1, characterized in that: In step (4), the sealing method is an immersion method: First, immerse the surface-treated coating into an inorganic rare earth sealing agent for 10 to 50 minutes (preferably 15 to 45 minutes, more preferably 20 to 40 minutes), so that the inorganic sealing agent penetrates into the pores of the coating and forms a neodymium-based rare earth conversion film on the surface of the coating, remove the coating, and dry it in air at room temperature for 1 to 6 hours (preferably 2 to 5 hours, more preferably 2 to 4 hours); Secondly, after inorganic sealing, the coating is immersed in an organic sealing agent for organic sealing and surface modification. The immersion time is 20 to 100 minutes (preferably 40-80 minutes, more preferably 50-70 minutes), and finally a drying and curing treatment is performed; the drying and curing treatment process is room temperature drying for 8-24 hours (preferably 10-16 hours, more preferably 12-14 hours), and finally a sealing coating is obtained.

7. An iron-based amorphous alloy coating sealing agent, characterized in that: Including inorganic sealants and organic sealants, The inorganic sealant is: 5-10 g (preferably 5-8 g) of neodymium nitrate and 10-15 ml (preferably 10-12 ml) of hydrogen peroxide (mass concentration 10-30%) dispersed in 500 ml of deionized water; The organic sealant is a mixture of butyl acetate and epoxy resin, wherein the amount of butyl acetate added is 75%-95% of the mass of the mixture; the mixture also contains 1H,1H,2H,2H-perfluorodecyltriethylsilane (FDTES), wherein the amount of FDTES added is 1%-3% of the mass of the organic sealant.

Citation Information

Patent Citations

  • Inorganic-organic compound hole sealing coating

    CN101654380A

  • Composite hole sealing agent for thermal sprayed coating and using method for composite hole sealing agent

    CN102925849A

  • High-temperature-resistant inorganic hole sealing agent for thermal spraying coating and preparation method of high-temperature-resistant inorganic hole sealing agent

    CN112694772A

  • Sealed sprayed coating, formation method thereof, and structural steelwork

    JP2018178238A