Copper target and grain orientation control method thereof
Through the multi-step process of cold forging, heat treatment, static pressure and cold rolling of copper castings, the grain size and orientation of copper targets are controlled, and the problem of insufficient control of grain size and orientation in the prior art is solved, and high purity is achieved Optimization of copper target materials is suitable for semiconductor integrated circuits above 12 inches.
Patent Information
- Application Number
- CN202411042058.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to effectively control the grain size and grain orientation of ultra-high purity copper targets, especially the grain proportion with a crystal plane index of <110> is insufficient, which cannot meet the requirements of semiconductor integrated circuits above 12 inches.
By sequentially performing cold forging, first heat treatment, static pressure treatment, cold rolling and second heat treatment, the deformation amount of static pressure and cold rolling is controlled, and the grain size and grain orientation of the copper target are controlled, so that the grain size and grain orientation of the copper target are controlled, so that The grain size is ≤20μm and the crystal plane index is <110> and the proportion is ≥40%.
It realizes effective control of the grain size and grain orientation of the copper target, meets the dual requirements of semiconductor integrated circuits, is simple to operate, low cost, and is suitable for industrial applications.
Smart Images

Figure BDA0004972636260000101 
Figure BDA0004972636260000111
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of target material preparation, and in particular to a copper target and a method for controlling grain orientation thereof. Background Art
[0002] With the increasing application of high-purity copper targets for integrated circuit interconnection, the purity, average particle size, particle size uniformity, and grain orientation of the targets are very stringent. First, the size of silicon wafers continues to increase, and the deposition area of the target film during the sputtering process continues to expand. In order to ensure the uniformity of each part of the film and the quality of fine wiring during the sputtering deposition process, according to the current development of the interconnection line process, the purity of copper and copper alloy targets must be controlled to above 6N. The higher the purity of the target, the better the quality of the sputtered film. Secondly, the average particle size and particle size uniformity of the target: when the grain size is within a certain range, the larger the grain size, the lower the deposition rate of the film. For copper and copper alloy targets, the smaller the grain size, the faster the sputtering rate during the sputtering process. The overall requirement for the grain is to make it as small as possible and to ensure the uniformity of the target grain size, which is very important for the thickness distribution of the deposited film. Finally, regarding the orientation of the target: the deposition rate of high-purity copper and copper alloy targets will be affected by the microscopic crystallographic orientation of the material. Within a certain grain size range, the more uniform the grain orientation, the better; copper and copper alloy targets for interconnects have relatively high requirements for grain orientation, which is also related to the life of the target. Related literature records that in the copper interconnection process, the finer and more uniform the grains of high-purity copper targets, the better the film quality. Too fine grains will speed up the film formation speed, reduce the life of the target, and increase the cost. Therefore, in terms of grain orientation, it is recorded that the densely packed direction of high-purity copper <110> The larger the proportion of crystal grains, the slower the sputtering rate is. This not only ensures the grain size and uniformity, but also greatly increases the service life of the target.
[0003] At present, the sputtering performance of ultra-high purity copper targets is mainly controlled by hot forging, rolling and heat treatment. However, the current process level can only control the grain size of ultra-high purity copper targets to 20-30μm, and the grain orientation is random, especially for those with a crystal plane index of <110> The proportion of grains is often less than 30%.
[0004] In summary, it is urgent to develop a method for controlling the grain orientation of ultra-high purity copper targets, reduce the grain size of ultra-high purity copper targets and increase the crystal plane index. <110> The grain ratio meets the dual requirements of grain size and grain orientation for semiconductor integrated circuits above 12 inches. Summary of the invention
[0005] The purpose of the present disclosure is to overcome the deficiencies of the prior art and provide a copper target and a method for controlling the grain orientation thereof.
[0006] To achieve the above objectives, the technical solution adopted by the present disclosure is: on the one hand, a method for controlling the grain orientation of a copper target is provided, comprising the following steps:
[0007] S1: cold forging the first copper casting to obtain a second copper casting;
[0008] S2: performing a first heat treatment on the second copper casting to obtain a third copper casting;
[0009] S3: subjecting the third copper casting to static pressure treatment to obtain a fourth copper casting; wherein the total deformation amount of the static pressure treatment is 40-90%;
[0010] S4: cold rolling the fourth copper casting and then subjecting it to a second heat treatment to obtain a copper target, wherein the total deformation amount of the cold rolling is 30-60%.
[0011] In some embodiments, in step S1, the cold forging adopts an upsetting and drawing deformation process, the upsetting deformation amount is 20-70%, and the drawing deformation amount is 50-100%.
[0012] In some embodiments, in step S2, the temperature of the first heat treatment is 150-200° C., and the time is 0.5-2 h.
[0013] In some embodiments, in step S3, the temperature of the static pressure treatment is 20-30°C.
[0014] In some embodiments, in step S4, the cold rolling pass deformation amount is 0.1-1%.
[0015] In some embodiments, in step S4, the cold rolling is cross rolling, and the rotation angle of the cross rolling is 30-60°.
[0016] In some embodiments, in step S4, the second heat treatment is performed at a temperature of 150-300° C. for a time of 2-5 hours.
[0017] In some embodiments, the purity of the first copper casting is 6N or above.
[0018] On the other hand, a copper target is provided, wherein the copper target is prepared by the method for controlling the grain orientation of the copper target.
[0019] In some embodiments, the copper target has a grain size of ≤20 μm and a crystal plane index of <110> The grain proportion is ≥40%.
[0020] Compared with the prior art, the beneficial effects of the present disclosure are as follows: the present disclosure sequentially processes the first copper casting through cold forging, the first heat treatment, static pressure treatment, cold rolling and the second heat treatment, and controls the deformation amount of static pressure treatment and cold rolling to control the grain size and grain orientation of the copper target, so that the grain size of the copper target is ≤20μm, and the crystal plane index is <110> The grain proportion is ≥40%, which meets the dual requirements of grain size and grain orientation for semiconductor integrated circuits above 12 inches. The grain orientation control method disclosed in the present invention is simple to operate, has low production cost, and is suitable for industrial application. DETAILED DESCRIPTION
[0021] In order to facilitate understanding of the present disclosure, the present disclosure will be described more fully below. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present disclosure more thorough and comprehensive.
[0022] As used herein:
[0023] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0024] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0025] When amount, concentration or other value or parameter is represented by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1-5", described range should be interpreted as including range "1-4", "1-3", "1-2", "1-2 and 4-5", "1-3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0026] In these examples, parts and percentages are by mass unless otherwise indicated.
[0027] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0028] “And / or” is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0029] The present disclosure provides a method for controlling the grain orientation of a copper target, comprising the following steps:
[0030] S1: cold forging the first copper casting to obtain a second copper casting;
[0031] S2: performing a first heat treatment on the second copper casting to obtain a third copper casting;
[0032] S3: subjecting the third copper casting to static pressure treatment to obtain a fourth copper casting; wherein the total deformation amount of the static pressure treatment is 40-90%;
[0033] S4: cold rolling the fourth copper casting and then subjecting it to a second heat treatment to obtain a copper target, wherein the total deformation amount of the cold rolling is 30-60%.
[0034] For example, in different embodiments, the total deformation amount of the static pressure treatment may be, but is not limited to, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%;
[0035] As in different embodiments, the total deformation of the cold rolling can be but is not limited to 30%, 32%, 35%, 37%, 40%, 43%, 45%, 48%, 50%, 52%, 55%, 58%, and 60%.
[0036] The present invention sequentially performs cold forging, first heat treatment, static pressure treatment, rolling and second heat treatment on the first copper casting to control the grain orientation in the first copper casting. The copper casting does not need to be cooled after the first heat treatment, but is directly subjected to static pressure treatment. The static pressure treatment is performed at the temperature of the first heat treatment, which promotes the grain orientation of the copper target to be <110> On the other hand, the grain size in the copper target can be refined; among them, cold forging and rolling can reduce the grain size, and rolling can further promote the grains in the copper target to have a crystal plane index of <110> The first heat treatment and the second heat treatment allow the grains to recrystallize and improve the uniformity of the grain size.
[0037] In addition, the total deformation of static pressure treatment and cold rolling will affect the grain orientation in the copper target. If the total deformation of static pressure treatment or the total deformation of cold rolling is too small, the crystal plane index in the copper target will be <110> The proportion of grains is small. If the total deformation of static pressure treatment or cold rolling is large, the crystal plane index in the copper target will be <110> The grain proportion is reduced and the distribution is uneven, which is not conducive to the subsequent use of the copper target.
[0038] In some embodiments, in step S1, the cold forging adopts an upsetting and drawing deformation process, the upsetting deformation amount is 20-70%, and the drawing deformation amount is 50-100%.
[0039] For example, in different embodiments, the deformation amount of the upsetting may be, but is not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%; preferably 25-50%;
[0040] For example, in different embodiments, the amount of deformation of the stretching may be, but is not limited to, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 100%, and is preferably 60-90%.
[0041] The disclosed cold forging by upsetting and stretching deformation process can not only avoid the problem of excessive grain growth caused by excessive temperature during hot forging, resulting in excessive grain size, but also promote grain refinement. In addition, by controlling the deformation amount during cold forging, the degree of grain refinement in the copper target can be further controlled.
[0042] In some embodiments, in step S2, the temperature of the first heat treatment is 150-200° C., and the time is 0.5-2 h.
[0043] As in different embodiments, the temperature of the first heat treatment may be, but is not limited to, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 200°C;
[0044] For example, in different embodiments, the time of the first heat treatment may be, but is not limited to, 0.5 h, 0.8 h, 1.0 h, 1.2 h, 1.5 h, 1.8 h, or 2.0 h.
[0045] Through the first heat treatment, the refined grains after cold forging are recrystallized, promoting the grain <110> The crystal plane arrangement increases the crystal plane index to <110> The proportion of grains.
[0046] In some embodiments, in step S3, the temperature of the static pressure treatment is 20-30°C.
[0047] For example, in different embodiments, the temperature of the static pressure treatment may be, but is not limited to, 20°C, 22°C, 24°C, 26°C, 28°C, or 30°C.
[0048] In some embodiments, in step S4, the cold rolling pass deformation amount is 0.1-1%.
[0049] For example, in different embodiments, the deformation amount of the cold rolling pass can be but is not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, and 1.0%.
[0050] In some embodiments, in step S4, the cold rolling is cross rolling, and the rotation angle of the cross rolling is 30-60°.
[0051] For example, in different embodiments, the rotation angle of the cross-rolling is 30°, 33°, 35°, 37°, 40°, 45°, 50°, 53°, 55°, 58°, or 60°.
[0052] The present invention further refines the grains of the copper target by controlling the deformation amount of the cold rolling pass to achieve the required grain size and ensure the consistency of the grain size of different batches of copper targets. In addition, the rotation angle of the cross rolling will result in a crystal plane index of <110> If the cross-rolling rotation angle is too small or too large, the crystal plane index may be <110> The grains are accumulated in a certain part of the copper target, making the crystal plane index in the copper target <110> The distribution uniformity of the grains decreases, and the crystal plane index is <110> The proportion of grains is reduced.
[0053] In some embodiments, in step S4, the second heat treatment is performed at a temperature of 150-300° C. for a time of 2-5 hours.
[0054] For example, in different embodiments, the temperature of the second heat treatment may be, but is not limited to, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C;
[0055] For example, in different embodiments, the time of the second heat treatment may be, but is not limited to, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, or 5 h.
[0056] The copper casting after rolling is subjected to the second heat treatment, which can refine the grains after rolling and recrystallize them, and promote the grains to <110> The crystal plane arrangement increases the crystal plane index to <110> The proportion of grains.
[0057] In some embodiments, the purity of the first copper casting is 6N or above.
[0058] For example, in different embodiments, the purity of the first copper casting may be, but is not limited to, 6N, 7N, and 8N. Specifically, the purity of the first copper casting being 6N or above means that the mass fraction of the first copper casting is above 99.9999%, and at this time, the purity of the first copper casting is extremely high, and the impurity content is below 1ppm; the ultra-high purity copper has a small grain boundary area, few internal lattice defects, and has excellent anti-electromigration ability, electrical conductivity, ductility, thermal conductivity, and corrosion resistance.
[0059] On the other hand, a copper target is provided, wherein the copper target is prepared by the method for controlling the grain orientation of the copper target.
[0060] In some embodiments, the copper target has a grain size of ≤20 μm and a crystal plane index of <110> The grain proportion is ≥40%.
[0061] Specifically, the grain size of the copper target may be, but is not limited to, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, and 20 μm;
[0062] The crystal face index is <110> The grain proportion is 40-60%, for example, it can be but not limited to 40%, 42%, 45%, 47%, 49%, 50%, 51%, 55%, 58%, 60%.
[0063] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0064] In the following examples, the purity of the first copper casting is 6N.
[0065] Example 1
[0066] This embodiment provides a method for controlling grain orientation of a copper target, comprising the following steps:
[0067] S1: The first copper casting is subjected to longitudinal upsetting and stretching treatment at room temperature by a forging press, wherein the deformation amount of the upsetting is 20% and the deformation amount of the stretching is 50%; thereby obtaining a second copper casting;
[0068] S2: subjecting the second copper casting to a first heat treatment at a temperature of 150° C. for 2 h to obtain a third copper casting;
[0069] S3: subjecting the third copper casting to static pressure treatment at a temperature of 20° C. and a total deformation of 40% to obtain a fourth copper casting;
[0070] S4: After cooling the fourth copper casting to room temperature, cold rolling is performed at room temperature by cross rolling, the rotation angle of the cross rolling is 30°, the pass deformation of the cold rolling is 1%, and the total deformation of the cold rolling is 30%;
[0071] The cold-rolled copper casting was subjected to a second heat treatment at a temperature of 150° C. for 5 h to obtain a copper target.
[0072] Example 2
[0073] This embodiment provides a method for controlling grain orientation of a copper target, comprising the following steps:
[0074] S1: The first copper casting is subjected to longitudinal upsetting and stretching treatment at room temperature by a forging press, wherein the deformation amount of the upsetting is 70% and the deformation amount of the stretching is 100%; thereby obtaining a second copper casting;
[0075] S2: subjecting the second copper casting to a first heat treatment at a temperature of 200° C. for 0.5 h, to obtain a third copper casting;
[0076] S3: subjecting the third copper casting to static pressure treatment at a temperature of 25° C. and a total deformation of 40% to obtain a fourth copper casting;
[0077] S4: After the fourth copper casting is cooled to room temperature, it is cold rolled by cross rolling at room temperature, the rotation angle of the cross rolling is 30°, the pass deformation of the cold rolling is 0.5%, and the total deformation of the cold rolling is 30%;
[0078] The cold-rolled copper casting was subjected to a second heat treatment at a temperature of 300° C. for 2 h to obtain a copper target.
[0079] Example 3
[0080] This embodiment provides a method for controlling grain orientation of a copper target, comprising the following steps:
[0081] S1: The first copper casting is subjected to longitudinal upsetting and stretching treatment at room temperature by a forging press, wherein the deformation amount of the upsetting is 50% and the deformation amount of the stretching is 75%; thereby obtaining a second copper casting;
[0082] S2: subjecting the second copper casting to a first heat treatment at a temperature of 180° C. for 1.5 h to obtain a third copper casting;
[0083] S3: subjecting the third copper casting to static pressure treatment at a temperature of 25° C. and a total deformation of 60% to obtain a fourth copper casting;
[0084] S4: After the fourth copper casting is cooled to room temperature, it is cold rolled by cross rolling at room temperature, the rotation angle of the cross rolling is 45°, the pass deformation of the cold rolling is 0.5%, and the total deformation of the cold rolling is 40%;
[0085] The cold-rolled copper casting was subjected to a second heat treatment at a temperature of 250° C. for 3 h to obtain a copper target.
[0086] Example 4
[0087] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S3, the total deformation amount of static pressure treatment is 40%; the remaining steps and parameters are the same as those in Embodiment 3.
[0088] Example 5
[0089] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S3, the total deformation amount of static pressure treatment is 50%; the remaining steps and parameters are the same as those in Embodiment 3.
[0090] Example 6
[0091] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S3, the total deformation amount of static pressure treatment is 75%; the remaining steps and parameters are the same as those in Embodiment 3.
[0092] Example 7
[0093] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S3, the total deformation amount of static pressure treatment is 90%; the remaining steps and parameters are the same as those in Embodiment 3.
[0094] Example 8
[0095] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S4, the total deformation amount of cold rolling is 30%; the remaining steps and parameters are the same as those in Embodiment 3.
[0096] Example 9
[0097] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S4, the total deformation amount of cold rolling is 50%; the remaining steps and parameters are the same as those in Embodiment 3.
[0098] Example 10
[0099] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S4, the total deformation amount of cold rolling is 60%; the remaining steps and parameters are the same as those in Embodiment 3.
[0100] Embodiment 11
[0101] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S4, the rotation angle of the cross-rolling is 30°; the remaining steps and parameters are the same as those in Embodiment 3.
[0102] Example 12
[0103] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S4, the rotation angle of the cross-rolling is 50°; the remaining steps and parameters are the same as those in Embodiment 3.
[0104] Embodiment 13
[0105] This embodiment provides a method for controlling the grain orientation of a copper target, which differs from Embodiment 3 only in that: in step S4, the rotation angle of the cross-rolling is 60°; the remaining steps and parameters are the same as those in Embodiment 3.
[0106] Comparative Example 1
[0107] This comparative example provides a method for controlling the grain orientation of a copper target, which differs from Example 3 only in that: in step S4, the rotation angle of the cross-rolling is 70°; the remaining steps and parameters are the same as those in Example 3.
[0108] Comparative Example 2
[0109] This comparative example provides a method for controlling the grain orientation of a copper target, which differs from Example 3 only in that: in step S4, the rotation angle of the cross-rolling is 20°; the remaining steps and parameters are the same as those in Example 3.
[0110] Comparative Example 3
[0111] This comparative example provides a method for controlling the grain orientation of a copper target, which differs from Example 3 only in that: in step S4, the total deformation amount of cold rolling is 65%; the remaining steps and parameters are the same as those in Example 3.
[0112] Comparative Example 4
[0113] This comparative example provides a method for controlling the grain orientation of a copper target, which differs from Example 3 only in that: in step S4, the total deformation amount of cold rolling is 25%; the remaining steps and parameters are the same as those in Example 3.
[0114] Comparative Example 5
[0115] This comparative example provides a method for controlling the grain orientation of a copper target, which differs from Example 3 only in that: in step S3, the total deformation amount of the static pressure treatment is 100%; the remaining steps and parameters are the same as those in Example 3.
[0116] Comparative Example 6
[0117] This comparative example provides a method for controlling the grain orientation of a copper target, which differs from Example 3 only in that: in step S3, the total deformation amount of the static pressure treatment is 30%; the remaining steps and parameters are the same as those in Example 3.
[0118] Performance Testing
[0119] The grain size and crystal plane index of the copper targets obtained in the above examples and comparative examples are <110> The specific method is as follows:
[0120] Grain size: measured according to the cross-section method disclosed in the national standard GB / T 6394-2017 "Method for determination of average grain size of metals";
[0121] The proportion of grains with (110) orientation was detected by electron backscattered diffraction (EBSD) mounted on a scanning electron microscope (SEM);
[0122] The test results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] It can be seen from the test results in Table 1 that the internal average grain size of the high-purity copper target prepared in Examples 1-13 of the present disclosure is small, and the crystal plane index is <110> The proportion of grains is more than 48%, and the grain distribution is uniform. Comparative Examples 1-6 make significant changes to the cross-rolling rotation angle, rolling deformation, and static pressure deformation, respectively, resulting in an increase in the average grain size inside the high-purity alloy copper target, an average grain size of more than 20um, and a crystal plane index of <110> The proportion of grains decreases, which reduces the relevant parameters of target preparation and cannot meet the use requirements.
[0127] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present disclosure rather than to limit the protection scope of the present disclosure. Although the present disclosure has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present disclosure can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present disclosure.
Claims
1. A method for controlling the grain orientation of a copper target, characterized in that: The following steps are involved: S1: cold forging the first copper casting to obtain a second copper casting; S2: performing a first heat treatment on the second copper casting to obtain a third copper casting; S3: subjecting the third copper casting to static pressure treatment to obtain a fourth copper casting; wherein the total deformation amount of the static pressure treatment is 40-90%; S4: The fourth copper casting is cold rolled and then subjected to a second heat treatment to obtain a copper target, wherein the total deformation amount of the cold rolling is 30-60%.
2. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: In step S1, the cold forging adopts an upsetting and drawing deformation process, the upsetting deformation amount is 20-70%, and the drawing deformation amount is 50-100%.
3. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: In step S2, the temperature of the first heat treatment is 150-200°C and the time is 0.5-2h.
4. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: In step S3, the temperature of the static pressure treatment is 20-30°C.
5. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: In step S4, the cold rolling has a deformation amount of 0.1-1%.
6. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: In step S4, the cold rolling is cross rolling, and the rotation angle of the cross rolling is 30-60°.
7. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: In step S4, the second heat treatment is performed at a temperature of 150-300°C and for a time of 2-5 hours.
8. The method for controlling the grain orientation of a copper target according to claim 1, characterized in that: The purity of the first copper casting is 6N or higher.
9. A copper target, characterized in that: The copper target is prepared by the method for controlling the grain orientation of the copper target according to any one of claims 1 to 8.
10. The copper target according to claim 9, characterized in that The grain size of the copper target is ≤20 μm, and the crystal plane index is <110> The grain proportion is ≥40%.