Method for preparing ethylene from flue gas of power plant through fused salt electrocatalytic reduction and preparation method of catalytic electrode

By using porous metal-ceramic composite electrodes in power plant flue gas for high-temperature molten salt electrochemical co-reduction, the problem of efficient utilization and low conversion efficiency in CCUS technology is solved, and high-throughput production of high-value ethylene is achieved.

CN118979268AActive Publication Date: 2024-11-19CHANGJIANG RIVER SCI RES INST CHANGJIANG WATER RESOURCES COMMISSION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411070783.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing CCUS technology lacks high-value utilization scenarios. The conversion efficiency of C2+ products such as ethylene is not high when the CO2 electrochemical reduction is used in room temperature, and it is difficult to achieve high-throughput capture and utilization in aqueous solution environments.

Method used

Metal-ceramic composite electrodes with high catalytic activity and porous structure were designed and prepared, and electrochemical co-reduction of CO2 and H2O in power plant flue gas was used to construct a rich three-phase reaction interface to improve CO2 conversion efficiency.

Benefits of technology

It realizes the direct conversion of CO2 and H2O in the medium and high-throughput of power plant flue gases into high-value ethylene products, overcomes the problems of high cost, high energy consumption and solid carbon products of traditional CCUS technology, and improves the conversion efficiency and product value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979268A_ABST
    Figure CN118979268A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon dioxide capture and utilization, and relates to a method for preparing ethylene through fused salt electrocatalytic reduction of flue gas of a power plant and a preparation method of a catalytic electrode. The porous metal-ceramic composite electrode for preparing the ethylene from the flue gas of the power plant through the fused salt electrocatalytic reduction is prepared and used as a catalytic electrode for preparing the ethylene from the flue gas of the power plant through the fused salt electrocatalytic reduction, and the characteristics that CO2 and H2O can be captured and electrochemical catalytic reduction can be achieved at the same time through the fused salt electrolyte are utilized; by constructing the porous metal-ceramic composite electrode with high catalytic activity, high-flux direct conversion of the flue gas of the power plant into a high-value ethylene product is realized. The problems that a traditional CCUS technology lacks a high-value application scene, the CO2 conversion efficiency is low in a normal-temperature water system environment, and solid carbon is easily generated due to direct molten salt electroreduction of CO2 are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon dioxide capture and utilization, and in particular to a method for preparing ethylene by electrocatalytic reduction of power plant flue gas through molten salt and a method for preparing a catalytic electrode. Background Art

[0002] Carbon dioxide capture, conversion and storage (CCUS) technology can achieve carbon dioxide emission reduction and utilization, and is one of the important strategic technologies to solve the low-carbon development of the coal-based energy system.

[0003] According to the capture location, power plant CO2 capture technology is usually divided into: pre-combustion capture, post-combustion capture, chemical chain capture and oxygen-enriched combustion. Chemical solvent absorption is the most well-researched and most widely used capture method in post-combustion capture technology. The so-called chemical absorption is to use alkaline solvents to selectively absorb CO2 in mixed flue gas, react to generate unstable salts, and then heat up in the desorption device to reversibly decompose and release CO2, thereby achieving CO2 removal and enrichment and solvent regeneration.

[0004] Carbon dioxide utilization technologies mainly include direct industrial utilization, geological utilization, chemical utilization, mineral utilization and biological utilization technology. CO2 direct industrial utilization technology is based on the physical properties of CO2 itself, and is used for the preservation, refrigeration, storage and transportation of food and vegetables. This technology is very mature, but the market capacity is relatively limited, and it is difficult to absorb the huge CO2 gas production of power plants. CO2 chemical utilization refers to the use of CO2 as a chemical raw material to produce chemical products. Typical chemical processes that require CO2 include: CO2 and methane dry reforming to prepare synthesis gas, CO2 through CO to prepare liquid fuel, CO2 hydrogenation to synthesize methanol, CO2 to synthesize dimethyl carbonate and other technologies. CO2 electrochemical conversion technology in aqueous solution system can reduce CO2 to high-value chemical products such as CO, methanol, ethylene, etc., and has broad prospects. CO2 electrochemical reduction technology in molten salt electrolyte can achieve CO2 capture and conversion in one step, but the conversion product is generally solid carbon.

[0005] Conventional CCUS technology has high amine absorbent consumption, high energy consumption in the desorption process, and narrow utilization pathways for captured CO2. Mature utilization technologies are significantly restricted by geographical factors. Therefore, the biggest challenges facing CCUS of flue gas from power plants are high cost, high energy consumption, and lack of high-value utilization technologies and scenarios. The electrocatalytic reduction of CO2 can directly convert CO2 into C 2+ High-value chemical products have significant technical and economic advantages. However, conventional CO2 electrocatalytic reduction currently occurs mostly in aqueous solution environment systems, which are difficult to achieve high-throughput conversion of CO2 and are difficult to directly use for the capture and utilization of CO2 in flue gas. At the same time, due to the limitations of thermodynamics and kinetics in normal temperature reaction environments, the CO2 conversion efficiency is not high. Summary of the invention

[0006] The present invention aims at the lack of high-value utilization scenarios of existing CCUS technology, and uses room-temperature CO2 electrochemical reduction to produce ethylene and other C 2 + The difficult problem of low product conversion efficiency is solved by designing and preparing a catalytic electrode with high catalytic activity, stability in a molten salt environment, and rich pores and a three-phase reaction interface, enhancing the selectivity and conversion efficiency of electrochemical reduction of CO2 and H2O in flue gas to ethylene, using the ability of high-temperature molten salt medium to capture and electrochemically convert CO2, and cleverly utilizing the current situation that power plant flue gas contains water vapor to achieve electrocatalytic co-reduction of CO2 and H2O in a molten salt electrolyte to produce ethylene, solving the problem of thermodynamic limitations of conventional CO2 electroreduction and the problem of solid carbon produced by molten salt electrochemical conversion of CO2. To this end, the present invention provides a method for preparing ethylene from power plant flue gas with molten salt electrocatalytic reduction and a method for preparing a catalytic electrode.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] One of the technical solutions of the present invention is to provide a method for preparing a porous metal-ceramic composite electrode for producing ethylene by electrocatalytic reduction of power plant flue gas from molten salt, the steps comprising:

[0009] The ceramic powder, the metal oxide powder, the dispersant, the organic monomer, the cross-linking agent and the water are mixed and ball-milled to obtain the metal ceramic slurry;

[0010] Adding a foaming agent to the metal ceramic slurry, and obtaining a foamed metal ceramic slurry after ball milling;

[0011] Adding an initiator and a catalyst to the foamed metal ceramic slurry, stirring, and then subjecting the slurry to tape casting, cross-linking and curing to obtain a ceramic body;

[0012] After drying the ceramic body, sintering is performed to obtain a porous metal ceramic electrode precursor;

[0013] The porous metal-ceramic electrode precursor is reduced at high temperature in a reducing atmosphere to obtain the porous metal-ceramic composite electrode.

[0014] Furthermore, the ceramic powder is an oxide conductive ceramic, preferably yttria-stabilized zirconia (YSZ), Gd-doped CeO2 (GDC) or a perovskite-based ceramic material, and has a particle size of 0.5 to 20 μm.

[0015] Furthermore, the metal oxide powder is CuO, and the particle size is 0.5 to 20 μm.

[0016] Preferably, the metal oxide powder further includes at least one of NiO, Fe3O4, CoO and MoO3, and has a particle size of 0.5 to 20 μm.

[0017] Furthermore, the mass ratio of the ceramic powder to the metal oxide powder is greater than 3:1.

[0018] Furthermore, the dispersant includes ammonium citrate or tetramethylammonium hydroxide, and the amount used is 0.5-2% of the mass of the ceramic powder.

[0019] Furthermore, the organic monomer is acrylamide, and the amount used is 0.5-15% of the mass of the ceramic powder.

[0020] Furthermore, the cross-linking agent is N,N-methylenebisacrylamide.

[0021] Furthermore, the mass ratio of the organic monomer to the cross-linking agent is 10:1.

[0022] Furthermore, the mass ratio of the ceramic powder to water is 3 to 8:1.

[0023] Furthermore, the foaming agent is at least one of triethanolamine dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide, and the amount used is 5-40% of the mass of water.

[0024] Furthermore, the initiator is an aqueous solution of ammonium persulfate, with a concentration of 5% to 10%, and an amount of 50 to 120% of the mass of the organic monomer.

[0025] Furthermore, the catalyst is N,N,N',N'-tetramethylethylenediamine, and the added amount is 0.01-1% of the mass of the ceramic powder.

[0026] Furthermore, the sintering temperature is 1000-1800° C., the heating rate is 5-20° C. / min, the holding time is 4-8 hours, and the sintering environment is an inert environment, preferably argon, nitrogen or vacuum.

[0027] Furthermore, the reducing atmosphere is a hydrogen atmosphere.

[0028] Furthermore, the high temperature reduction is carried out at a temperature of 800 to 1000° C. and for a time of 1 to 4 hours.

[0029] After high-temperature reduction in a reducing atmosphere, the metal component in the catalytic electrode is metal Cu, Cu-Ni alloy, Cu-Fe alloy, Cu-Co alloy, Cu-Mo alloy, Cu-Ni-Fe alloy, Cu-Ni-Co alloy or Cu-Fe-Co alloy.

[0030] The second technical solution of the present invention is to provide a porous metal-ceramic composite electrode prepared by the above method.

[0031] The third technical solution of the present invention is to provide an application of the above-mentioned porous metal-ceramic composite electrode as a catalytic electrode in the production of ethylene by molten salt electrocatalytic reduction of power plant flue gas.

[0032] Technical solution 4 of the present invention: Provided is a method for producing ethylene by electrocatalytic reduction of power plant flue gas using molten salt, the steps comprising:

[0033] The cathode and anode are immersed in an electrolyte to construct a two-electrode system, and electric field flue gas is introduced into the cathode to obtain ethylene product through electrolysis;

[0034] The electrolyte comprises a molten salt electrolyte and an additive;

[0035] The cathode is the porous metal-ceramic composite electrode.

[0036] Furthermore, the additive is at least one of an additive containing oxygen ions, an additive containing hydroxide ions or an additive containing borate ions, and the amount used is 3 to 20% of the mass of the molten salt electrolyte.

[0037] Preferably, the additive containing oxygen ions includes at least one of Li2O, Na2O, K2O and CaO; the additive containing hydroxide ions includes at least one of LiOH, NaOH, KOH and Ca(OH)2; the additive containing borate ions includes at least one of sodium borate, sodium metaborate, sodium polyborate, potassium borate and calcium borate.

[0038] Furthermore, the molten salt electrolyte includes carbonate, chloride salt or hydroxide of alkali metal or alkaline earth metal.

[0039] Preferably, the carbonate is at least one of Li2CO3, Na2CO3, K2CO3 and CaCO3; the chloride salt is at least one of LiCl, NaCl, KCl and CaCl2; and the hydroxide is at least one of LiOH, NaOH, KOH or Ca(OH)2.

[0040] The melting point or eutectic point of the molten salt electrolyte used in the present invention is about 400-1000°C, and the chemical properties remain stable and do not decompose at about 400-1000°C.

[0041] More preferably, the molten salt electrolyte is Li2CO3, Na2CO3 and K2CO3, with a molar ratio of 43.5:31.5:25.

[0042] The melting point of the above three carbonate mixture is 393℃.

[0043] Furthermore, the electrolysis is constant current electrolysis or constant voltage electrolysis.

[0044] Preferably, the current of the constant current electrolysis is 50mA to 2A.

[0045] Preferably, the voltage of the constant voltage electrolysis is 1.5V to 5V.

[0046] Furthermore, the anode is one of Au, Pt, tin dioxide ceramic, graphite or platinum-plated titanium precious metal coated electrodes, or one of metal-based oxide coated electrodes of nickel and its alloys, iron and its alloys, copper and its alloys, chromium and its alloys or aluminum and its alloys.

[0047] Furthermore, the working temperature of the electrolyte is 400-1000°C.

[0048] Furthermore, the electric field flue gas includes CO2 and H2O.

[0049] Furthermore, the structure of the anode is a sheet or mesh structure.

[0050] High-temperature alkaline molten salt media can efficiently capture CO2, thanks to the rich oxygen ions (O 2- ). At the same time, molten salt as an electrolyte has the ability to in-situ electrochemical conversion and utilization of CO2. However, at the same time, due to the thermodynamic conditions for obtaining gas phase products and the composition structure of the reaction electrode, the products of conventional molten salt electrochemical conversion of CO2 are mainly solid carbon materials. Considering that the flue gas emitted by power plants contains a large amount of water vapor, H2O can be used as an oxidant and hydrogen source to undergo a co-reduction reaction with CO2 at the cathode to promote the coupling production of ethylene products. The corresponding electrode reactions are as follows:

[0051] 2CO2+2H2O+12e - =C2H4+6O 2-

[0052] In particular, in order to simultaneously realize the electrochemical conversion of CO2 and H2O in power plant flue gas by molten salt, a reaction electrode with catalytic ability is specially designed. The catalytic electrode needs to have abundant active sites for catalyzing the co-reduction of CO2 and H2O to produce ethylene, and the active sites need to be able to remain stable in a high-temperature molten salt environment and reduction potential. In addition, a rich interconnected pore structure needs to be constructed in the electrode structure to help construct a gas-liquid-solid three-phase catalytic reaction interface. Metallic copper and its alloys have excellent activity in catalyzing the electrochemical reduction of CO2 to produce ethylene.

[0053] The present invention discloses the following technical effects:

[0054] The metal active sites of the porous metal-ceramic composite electrode prepared by the present invention have excellent catalytic ability. They are precipitated in situ from the ceramic interface and anchored on the ceramic surface. Compared with metal elements, they have stronger stability and can cope with harsh high-temperature molten salt environments to avoid corrosion. Secondly, the interaction between the metal and ceramic interfaces constructs a new catalytic reaction interface, enhancing the CO2 conversion ability. Finally, the porous structure promotes the construction and exposure of the three-phase reaction interface, enhancing the mass transfer process of the electrocatalytic reaction.

[0055] The present invention utilizes the characteristics of molten salt electrolyte that can simultaneously capture and electrochemically catalytically reduce CO2 and H2O, and constructs a porous metal-ceramic composite electrode with high catalytic activity to directly convert power plant flue gas into high-value ethylene products at high flux. This overcomes the problem of traditional CCUS technology lacking high-value application scenarios, the problem of low CO2 conversion efficiency under normal temperature water environment, and the problem that direct molten salt electroreduction of CO2 easily produces solid carbon. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0057] Figure 1 This is a scanning electron microscope image of the Cu / Ni-YSZ precursor;

[0058] Figure 2 This is a scanning electron microscope image of Cu / Ni-YSZ;

[0059] Figure 3 Mercury injection test data of Cu / Ni-YSZ;

[0060] Figure 4 is a graph showing changes in ethylene concentration of gas phase products in Example 2, Comparative Example 1 and Comparative Example 2;

[0061] Figure 5 This is a scanning electron microscope image of the Cu / Ni-YSZ electrode after 5 hours of electrolysis;

[0062] Figure 6 This is a scanning electron microscope image of the electrode surface of Control Example 1;

[0063] Figure 7 This is the XRD diagram of the solid product on the electrode surface of Control Example 1. DETAILED DESCRIPTION

[0064] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0065] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0066] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0067] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0068] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0069] Example 1

[0070] The preparation steps of the porous metal-ceramic composite electrode are as follows:

[0071] S1, mixing YSZ ceramic powder, CuO powder, NiO powder, dispersant (ammonium citrate), organic monomer (acrylamide), crosslinking agent (N,N-methylenebisacrylamide) and water and ball milling to obtain a stable metal ceramic slurry;

[0072] The particle size of YSZ ceramic powder and metal oxide powder (CuO powder and NiO powder) is less than 10 μm, the mass ratio is 4:1, the molar ratio of NiO and CuO is 1:1, the dispersant is 2% of the mass of the YSZ ceramic powder, the organic monomer is 5% of the mass of the YSZ ceramic powder, the mass ratio of the organic monomer to the cross-linking agent is 10:1, and the mass ratio of the YSZ ceramic powder to water is 5:1.

[0073] S2, adding a foaming agent (sodium dodecyl sulfate) to the metal ceramic slurry, and obtaining a foamed metal ceramic slurry after ball milling; the amount of the foaming agent is 20% of the mass of the water added in step S1;

[0074] S3, adding an initiator (aqueous solution of ammonium persulfate with a concentration of 5%) and a catalyst (N,N,N',N'-tetramethylethylenediamine) to the foamed metal ceramic slurry, stirring and then tape-casting the ceramic slurry, and curing the ceramic slurry after cross-linking the organic monomer to obtain a sheet-like ceramic body; the amount of the initiator added is 50% of the mass of the organic monomer in step S1, and the amount of the catalyst added is 0.05% of the mass of the YSZ ceramic powder in step S1;

[0075] S4, drying the flaky ceramic body, and then sintering at high temperature to obtain a porous metal ceramic electrode precursor, denoted as Cu / Ni-YSZ precursor; the sintering temperature is 1300°C, the heating rate is 10°C / min, the holding time is 8h, and the sintering environment is nitrogen;

[0076] S5. Reduce the porous metal-ceramic electrode precursor at 800° C. for 2 h in a hydrogen atmosphere to precipitate the metal component from the ceramic surface in situ, thereby obtaining a porous metal-ceramic composite electrode, which is recorded as Cu / Ni-YSZ.

[0077] Figure 1 This is a scanning electron microscope image of the Cu / Ni-YSZ precursor; Figure 2 This is a scanning electron microscope image of Cu / Ni-YSZ. Figure 1 and Figure 2 It can be seen that NiO and CuO are reduced to metal elements and form alloys in a hydrogen atmosphere. Cu-Ni nanoalloy particles are precipitated from the YSZ surface and anchored on the YSZ surface, thereby enhancing the corrosion resistance of the nanoparticles. A two-phase interface between metal nanoparticles and YSZ is formed, which can serve as an active site for catalytic reactions.

[0078] Figure 3 The mercury injection test data of Cu / Ni-YSZ is given by Figure 3 It can be seen that Cu / Ni-YSZ has obvious pore structure in the pore size range of 1000-2000nm and 10000-50000nm, proving that it is a porous structure.

[0079] Example 2

[0080] A method for preparing ethylene by electrocatalytic reduction of flue gas from a power plant using molten salt, comprising the following steps:

[0081] S1. Preparation of electrolyte: 500 g of a mixed salt of three carbonates, Li2CO3, Na2CO3 and K2CO3, with a molar ratio of 43.5:31.5:25, the melting point of the three carbonate mixture is 393° C., and placed in an alumina crucible, and then 15 g of Li2O additive is added, the electrolyte operating temperature range is about 700° C., and an electrolyte is obtained;

[0082] S2, a two-electrode system consisting of a cathode (Cu / Ni-YSZ prepared in Example 1) and an anode (metal Pt sheet), wherein the electrode materials are immersed in an electrolyte;

[0083] S3. Directly introduce the desulfurized and denitrified flue gas (containing 15% CO2 and 20% H2O, the rest is nitrogen) into the cathode surface immersed in the molten salt. At the same time, electrolysis is performed at a constant cell voltage of 2.0V. The gas phase product obtained is ethylene. The gas phase product is monitored by an online gas analyzer. The data is as follows: Figure 4 shown.

[0084] Figure 5 This is a scanning electron microscope image of the Cu / Ni-YSZ electrode after 5 hours of electrolysis. Figure 5 It can be seen that even after five hours of electrolysis, the Cu-Ni metal nanoparticles can still be clearly distinguished from the electrode surface, indicating their good corrosion resistance and structural stability under electrolysis conditions.

[0085] Comparative Example 1

[0086] Compared with Example 1, the only difference is that the flue gas from the power plant is replaced by an equal amount of dry CO2 gas. The data on the change in ethylene product concentration are as follows: Figure 4 shown.

[0087] Figure 6 This is a scanning electron microscope image of the electrode surface of control example 1. Figure 6 It can be seen that the product is in a solid state. Figure 4 The ethylene concentration in the solution is 0.

[0088] Figure 7 The XRD diagram of the solid product on the electrode surface of Control Example 1 is shown in Figure 7 It can be seen that the solid product only has a diffraction peak at about 25°, which corresponds to the diffraction peak of amorphous carbon, proving that the solid product is solid carbon.

[0089] Comparative Example 2

[0090] Compared with Example 1, the only difference is that the cathode is replaced with a single copper sheet. The ethylene product concentration change data is as follows: Figure 4 shown.

[0091] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a porous metal-ceramic composite electrode for preparing ethylene from power plant flue gas by molten salt electrocatalytic reduction, characterized in that the steps include: The ceramic powder, the metal oxide powder, the dispersant, the organic monomer, the cross-linking agent and the water are mixed and ball-milled to obtain the metal ceramic slurry; Adding a foaming agent to the metal ceramic slurry, and obtaining a foamed metal ceramic slurry after ball milling; Adding an initiator and a catalyst to the foamed metal ceramic slurry, stirring, and then subjecting the slurry to tape casting, cross-linking and curing to obtain a ceramic body; After drying the ceramic body, sintering is performed to obtain a porous metal ceramic electrode precursor; The porous metal-ceramic electrode precursor is reduced at high temperature in a reducing atmosphere to obtain the porous metal-ceramic composite electrode.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the ceramic powder and the metal oxide powder is greater than 3:1; the amount of the dispersant is 0.5-2% of the mass of the ceramic powder; the amount of the organic monomer is 0.5-15% of the mass of the ceramic powder; the mass ratio of the organic monomer to the cross-linking agent is 10:1; the mass ratio of the ceramic powder to water is 3-8:1; the amount of the foaming agent is 5-40% of the mass of water; the amount of the initiator is 50-120% of the mass of the organic monomer; the amount of the catalyst added is 0.01-1% of the mass of the ceramic powder; the sintering temperature is 1000-1800°C, the heating rate is 5-20°C / min, the insulation time is 4-8h, and the sintering environment is an inert environment; the temperature of the high-temperature reduction is 800-1000°C, and the time is 1-4h.

3. The preparation method according to claim 1, characterized in that: The ceramic powder is oxide conductive ceramic; the metal oxide powder is CuO; the dispersant includes ammonium citrate or tetramethylammonium hydroxide; the organic monomer is acrylamide; the cross-linking agent is N,N-methylenebisacrylamide; the foaming agent is at least one of triethanolamine dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide; the initiator is an aqueous solution of ammonium persulfate with a concentration of 5% to 10%; and the catalyst is N,N,N',N'-tetramethylethylenediamine.

4. The preparation method according to claim 3, characterized in that: The metal oxide powder also includes at least one of NiO, Fe3O4, CoO and MoO3; the oxide conductive ceramic is YSZ, GDC or perovskite-based ceramic material.

5. A porous metal-ceramic composite electrode prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the porous metal-ceramic composite electrode as claimed in claim 5 as a catalytic electrode in the production of ethylene from molten salt electrocatalytic reduction of flue gas in power plants.

7. A method for preparing ethylene from power plant flue gas by electrocatalytic reduction of molten salt, characterized in that the steps include: The cathode and anode are immersed in an electrolyte to construct a two-electrode system, and electric field flue gas is introduced into the cathode to obtain ethylene product through electrolysis; The electrolyte comprises a molten salt electrolyte and an additive; The cathode is the porous metal-ceramic composite electrode as claimed in claim 5.

8. The method according to claim 7, characterized in that The additive is at least one of an additive containing oxygen ions, an additive containing hydroxide ions or an additive containing borate ions, and the amount used is 3 to 20% of the mass of the molten salt electrolyte; the molten salt electrolyte includes carbonates, chloride salts or hydroxides of alkali metals or alkaline earth metals; and the electrolysis is constant current electrolysis or constant voltage electrolysis.

9. The method according to claim 8, characterized in that The additive containing oxygen ions includes at least one of Li2O, Na2O, K2O and CaO; the additive containing hydroxide ions includes at least one of LiOH, NaOH, KOH and Ca(OH)2; the additive containing borate ions includes at least one of sodium borate, sodium metaborate, sodium polyborate, potassium borate and calcium borate; the carbonate is at least one of Li2CO3, Na2CO3, K2CO3 and CaCO3; the chloride salt is at least one of LiCl, NaCl, KCl and CaCl2; the hydroxide is at least one of LiOH, NaOH, KOH or Ca(OH)2; the current of the constant current electrolysis is 50mA~2A; the voltage of the constant voltage electrolysis is 1.5V~5V.

10. The method according to claim 7, characterized in that The anode is one of Au, Pt, tin dioxide ceramic, graphite or platinum-plated titanium precious metal coating electrodes, or one of metal-based oxide coating electrodes of nickel and its alloys, iron and its alloys, copper and its alloys, chromium and its alloys or aluminum and its alloys; the working temperature of the electrolyte is 400-1000°C; the electric field flue gas includes CO2 and H2O.

Citation Information

Patent Citations

  • Method for preparing carbon-containing compound by electro-catalyzing carbon dioxide with copper alloy material

    CN111074294A

  • Method for improving carbon dioxide conversion rate during electrolytic reduction of carbon dioxide by using electrolysis system

    CN113430539A

  • CuO-CeO2 nano-catalyst rich in oxygen vacancies, preparation method of CuO-CeO2 nano-catalyst and application of CuO-CeO2 nano-catalyst in electrocatalytic carbon dioxide reduction

    CN115627494A

  • Ceramic electrode with 3D (three-dimensional) communicating hole structure and preparation method of ceramic electrode

    CN116732555A

  • Catalyst as well as preparation method and application thereof

    CN117418269A