Copper-based nano material with bead-shaped series structure, electrode and preparation method and application of copper-based nano material
By preparing copper-based nanomaterials with bead-like tandem structures and applying them to electrodes, the problem of low catalytic activity of Cu-based catalysts was solved, achieving efficient generation of multi-carbon products and providing a new research direction for CO2RR.
Patent Information
- Application Number
- CN202411059101.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-17
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Existing Cu-based catalysts exhibit low catalytic activity and low current density during electrocatalytic CO2 reduction, making it difficult to efficiently generate high-value multi-carbon products.
Copper-based nanomaterials with bead-like tandem structures were prepared by reacting sodium borohydride, CuCl2·2H2O and Ce(NO3)3·6H2O in a solvent in a specific ratio to form copper-based nanomaterials, which were then applied to electrodes and combined with an electrolytic cell for CO2RR.
The copper-based nanomaterials, which achieve highly selective generation of multi-carbon products at high current densities, are simple to prepare, low in cost, and exhibit good catalytic activity, providing a new research direction for CO2RR.
Smart Images

Figure CN118979276A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic materials, and in particular to a copper-based nano material with a bead-like series structure, an electrode, and a preparation method and application thereof. Background Art
[0002] Excessive emissions of the greenhouse gas carbon dioxide (CO2) can easily cause a series of energy and environmental problems. Electrocatalytic CO2 reduction (CO2RR) can be combined with new energy power generation technology to achieve the recycling of carbon resources.
[0003] Among all the products of CO2RR, multi-carbon products (C 2+ ) has attracted much attention from researchers due to its high added value and wide applicability. However, due to the involvement of multiple electron transfers and competing reactions (hydrogen evolution reaction), C 2+ The selectivity and yield of the products remain challenging. So far, a variety of metals have been explored to promote the CO2RR to C 2+ products, among which copper (Cu) can convert CO2 into C through more than two electron transfer mechanisms. 2+ The product has a significant Faraday efficiency (FE), so it has attracted much attention. A large number of experiments and theories have proved that Cu-based catalysts can enhance the adsorption of *CO intermediates due to their unique electronic structure and further promote CC coupling, which can efficiently convert CO2 into high-value multi-carbon products. Studies have shown that Cu-based catalysts still have problems such as low catalytic activity and low current density. Therefore, designing and preparing catalysts with high activity and high selectivity is an important challenge for CO2RR.
[0004] Therefore, the present invention develops a copper-based nanomaterial with a bead-like series structure having a simple preparation method and excellent performance. Summary of the invention
[0005] The purpose of the present invention is to provide a copper-based nanomaterial with a bead-like series structure and a preparation method thereof in view of the technical defects existing in the prior art.
[0006] Another object of the present invention is to provide the copper-based nanomaterial for use as a catalyst in an electrode.
[0007] Another object of the present invention is to provide an electrode based on the copper-based nanomaterial.
[0008] Another object of the present invention is to provide an electrolytic cell based on the electrode.
[0009] Another object of the present invention is a method for preparing multi-carbon products using the electrolytic cell.
[0010] The technical solution adopted to achieve the purpose of the present invention is:
[0011] A copper-based nanomaterial with a bead-like serial structure is prepared by the following method:
[0012] Sodium borohydride is dispersed in a solvent to form a solution A, CuCl2·2H2O and Ce(NO3)3·6H2O are dissolved in a solvent to form a solution B, solution B is added to solution A under stirring conditions to react to obtain a precipitate, which is then washed, centrifuged and dried to obtain the copper-based nanomaterial.
[0013] In the above technical solution, the solvent for dissolving the sodium borohydride is water, and the solvent for dissolving the CuCl2·2H2O and Ce(NO3)3·6H2O is ethanol.
[0014] In the above technical solution, the molar ratio of sodium borohydride, CuCl2·2H2O and Ce(NO3)3·6H2O is (9-11):(1.7-1.9):(0.05-0.07).
[0015] In the above technical solution, the reaction time is 30-60 minutes and the reaction temperature is 20-30°C.
[0016] In the above technical solution, ultrapure water is used for washing and freeze drying is performed in a freeze dryer, and the freeze drying time is 10-15 hours.
[0017] Another aspect of the present invention also includes the use of the copper-based nanomaterial as a catalyst in an electrode.
[0018] Another aspect of the present invention also includes an electrode based on copper-based nanomaterials, wherein the electrode is prepared by the following method:
[0019] The copper-based nanomaterial is ground and then dispersed in methanol, and Nafion solution is added to obtain a dispersion after ultrasonic dispersion is uniform. The dispersion is evenly coated on the carbon layer side of the hydrophobic carbon paper and naturally air-dried to obtain the electrode.
[0020] In the above technical solution, the loading amount of the copper-based nanomaterial per square centimeter is 1.2-1.4 mg.
[0021] Another aspect of the present invention also includes an electrolytic cell, which includes an electrochemical workstation and a working electrode chamber and a counter electrode chamber separated by an anion exchange membrane. The electrode of the copper-based nanomaterial is used as the working electrode, the reference electrode is an Ag / AgCl electrode, and the counter electrode is a Pt sheet.
[0022] Another aspect of the present invention also includes a method for preparing multi-carbon products by CO2RR using the electrolytic cell, wherein the working electrode chamber and the counter electrode chamber both use a saturated KOH solution as an electrolyte, carbon dioxide is introduced into the electrolyte of the working electrode chamber until saturated, and the electrolyte is heated at 250-450 mA cm -2 At a current density of 1.5 Å, polycarbonate is formed by electrolysis.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The copper-based nanomaterial of the present invention can realize the generation of multi-carbon products with high selectivity under high current density. The preparation method of the copper-based nanomaterial is simple, easy to operate, low cost, and the prepared nanomaterial has good catalytic activity.
[0025] 2. The copper-based nanomaterials of the present invention have opened up a new research direction in the electrocatalytic conversion of carbon dioxide into multi-carbon products, providing assistance for achieving efficient CO2RR. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the XRD pattern of Cu / Ce2O3 and Cu / Cu2O;
[0027] Figure 2 It is the SEM image of Cu / Ce2O3;
[0028] Figure 3 This is the TEM image of Cu / Ce2O3;
[0029] Figure 4 is the Faradaic efficiency diagram of all products of CO2RR catalyzed by Cu / Ce2O3;
[0030] Figure 5 This is the Faraday efficiency diagram of multi-carbon products in CO2RR catalyzed by Cu / Ce2O3.
[0031] Figure 6 is the Faradaic efficiency diagram of all products of CO2RR catalyzed by Cu / Cu2O;
[0032] Figure 7 This is the Faraday efficiency diagram of multi-carbon products in CO2RR catalyzed by Cu / Cu2O. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0034] Example 1
[0035] A copper-based nanomaterial with a bead-like series structure is prepared by the following steps:
[0036] First, 10mmol of sodium borohydride was dissolved and dispersed in 20ml of ultrapure water to form solution A, and then 306.86mg of CuCl2·2H2O and 26.1mg of Ce(NO3)3·6H2O were weighed and dissolved in 20ml of ethanol to form solution B. Solution B was slowly poured into the stirring solution A, and the two were mixed and stirred on a magnetic stirrer at room temperature for 40min to obtain a black precipitate. The obtained sample was washed and centrifuged with ultrapure water several times to remove excess sodium borohydride (centrifuge parameters: 10000r / min, 5min), and finally the sample was placed in a freeze dryer and vacuum freeze-dried for 12h and then taken out to finally obtain a black bead-like tandem copper-based nanomaterial, recorded as Cu / Ce2O3.
[0037] XRD test was performed on the Cu / Ce2O3 obtained in Example 1:
[0038] In order to more scientifically determine the phase in the reaction process, the material was subjected to X-ray powder diffraction (XRD) test. The test results are as follows: Figure 1 As shown in the figure, the XRD spectrum shows obvious peaks at 43.3°, 50.4°, and 74.1°, which match the standard peaks of metal Cu and correspond to the (111), (200), and (220) planes of Cu, respectively. Cu and Ce2O3 coexist in the XRD spectrum of Cu / Ce2O3, indicating the successful synthesis of the Cu / Ce2O3 catalyst.
[0039] The Cu / Ce2O3 obtained in Example 1 was characterized by morphology:
[0040] High-resolution scanning electron microscopy (SEM) and high-resolution transmission electron microscopy (TEM) images clearly show that Cu / Ce2O3 is in a bead-like series structure.
[0041] Example 2
[0042] The material obtained in Example 1 was subjected to electrochemical testing.
[0043] The electrochemical tests were carried out on an electrochemical workstation (CHI 1140E) at 250-450 mA cm -2 The CO2RR performance was tested within a current density range.
[0044] The electrochemical CO2RR performance test system of this embodiment adopts a mobile phase electrolytic cell, and the working electrode chamber and the counter electrode chamber are separated by an anion exchange membrane. Both electrode chambers use a 1M saturated KOH solution (pH=14) as the electrolyte. The reference electrode uses an Ag / AgCl electrode, and the counter electrode uses a Pt sheet (2cm×2cm). Carbon dioxide is introduced into the electrolyte of the working electrode chamber until it is saturated, and an electrolytic reaction is carried out, and CO2RR obtains a multi-carbon compound.
[0045] The gaseous products of CO2RR were tested by Shimadzu gas chromatography (GC-2014), and the liquid products were qualitatively analyzed by nuclear magnetic resonance spectrometer, heavy water was used as the deuterium ion source, and dimethyl sulfoxide (DMSO) was used as the internal standard. The test results are as follows Figure 4-Figure 5 As shown, the gas phase product results show that the main product is C2H4, and H2 appears in very small amounts as a by-product of CO2RR. There are four liquid phase products, namely HCOOH, CH3COOH, C2H5OH and C3H7OH, among which C2H5OH is the main liquid phase product. Figure 4 The three light colors at the bottom of the middle column represent the three C1 products, namely carbon monoxide (CO), hydrogen (H2) and formic acid (HCOOH), and the four dark blocks at the top represent the four C 2+ The products are ethylene (C2H4), acetic acid (CH3COOH), ethanol (C2H5OH) and isopropanol (C3H7OH). Figure 5 It can be seen that with the increase of potential, the C2 product gradually increases. -2 At a current density of 2+ The Faradaic efficiency of the product reaches 70%, of which C2H4 accounts for 48%.
[0046] Comparative Example 1
[0047] A Cu / Cu2O composite material is synthesized by liquid phase chemical reduction reaction, and the preparation method comprises the following steps:
[0048] First, 10mmol of sodium borohydride was dissolved and dispersed in 20ml of ultrapure water to form solution A, and then 306.86mg of CuCl2·2H2O was weighed and dissolved in 20ml of ethanol to form solution B. Solution B was slowly poured into the stirring solution A, and after the two were mixed, they were stirred on a magnetic stirrer at room temperature for 40 minutes to obtain a black precipitate. The obtained sample was washed and centrifuged with ultrapure water several times to remove excess sodium borohydride (centrifuge parameters: 10000r / min, 5min), and finally the sample was placed in a freeze dryer and vacuum freeze-dried for 12h and then taken out to finally obtain a black Cu / Cu2O composite material, recorded as Cu / Cu2O. The XRD pattern of Cu / Cu2O is shown in Figure 1 shown.
[0049] Comparative Example 2
[0050] The material obtained in Comparative Example 2 was subjected to electrochemical testing using the same method as in Example 2. The results are as follows: Figure 6-7 As shown, it can be seen from the comparison between Example 2 and Comparative Example 2 that at 400 mA cm -2At a current density of , the Faraday efficiency of multi-carbon products increased by 3.5 times after adding the Ce component.
[0051] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A copper-based nanomaterial with a bead-like series structure, characterized in that: Prepared by the following method: Sodium borohydride is dispersed in a solvent to form a solution A, CuCl2·2H2O and Ce(NO3)3·6H2O are dissolved in a solvent to form a solution B, solution B is added to solution A under stirring conditions to react to obtain a precipitate, which is then washed, centrifuged and dried to obtain the copper-based nanomaterial.
2. The copper-based nanomaterial with a bead-like serial structure as claimed in claim 1, characterized in that: The solvent for dissolving the sodium borohydride is water, and the solvent for dissolving the CuCl2·2H2O and Ce(NO3)3·6H2O is ethanol.
3. The copper-based nanomaterial with a bead-like serial structure as claimed in claim 1, characterized in that: The molar ratio of sodium borohydride, CuCl2·2H2O and Ce(NO3)3·6H2O is (9-11):(1.7-1.9):(0.05-0.07).
4. The copper-based nanomaterial with a bead-like serial structure as claimed in claim 1, characterized in that: The reaction time is 30-60 minutes, and the reaction temperature is 20-30°C.
5. The copper-based nanomaterial with a bead-like serial structure as claimed in claim 1, characterized in that: The mixture was washed with ultrapure water and freeze-dried in a freeze dryer for 10-15 hours.
6. Use of the copper-based nanomaterial with a bead-like serial structure as claimed in claim 1 as a catalyst in an electrode.
7. An electrode based on copper-based nanomaterials, characterized in that: The electrode is prepared by the following method: The copper-based nanomaterial as claimed in claim 1 is ground and then dispersed in methanol, and Nafion solution is added to obtain a dispersion after ultrasonic dispersion is uniform. The dispersion is evenly coated on the carbon layer side of the hydrophobic carbon paper and naturally air-dried to obtain the electrode.
8. The electrode according to claim 7, characterized in that The loading amount of copper-based nanomaterials per square centimeter is 1.2-1.4 mg.
9. An electrolytic cell, characterized in that The electrolytic cell comprises an electrochemical workstation and a working electrode chamber and a counter electrode chamber separated by an anion exchange membrane, the electrode of the copper-based nanomaterial as claimed in claim 7 is used as the working electrode, the reference electrode is an Ag / AgCl electrode, and the counter electrode is a Pt sheet.
10. A method for preparing multi-carbon products by CO2RR using the electrolytic cell according to claim 9, characterized in that: The working electrode chamber and the counter electrode chamber both use saturated KOH solution as the electrolyte. Carbon dioxide is introduced into the electrolyte of the working electrode chamber until it is saturated. -2 At a current density of 1.5 Å, polycarbonate is formed by electrolysis.