Production process for preparing polyester yarn from short fibers
Through the use of layered alternating mixing and automatic laying equipment, combined with environmentally friendly finishing agents and low-temperature vacuum drying technology, the problems of uneven fiber distribution and unstable performance in polyester yarns made from staple fibers are solved, and high strength and high Yarn production with breathability and high color fastness meets the needs of high-end textiles.
Patent Information
- Application Number
- CN202411048297.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
In the existing production process of polyester yarn made of staple fiber, the blend ratio is determined without scientificity and the fiber distribution is uneven, resulting in unstable yarn performance, which cannot meet the high-strength, high breathability, high dyeing uniformity and high quality of high-end textiles. Color fastness requirement.
Blends by layered alternating mixing, combining pre-humidification, fiber length and fineness classification, using automatic laying equipment and ultrasonic assisted blending, and real-time monitoring of tension during spinning, and using environmentally friendly finishing agents and low-temperature vacuum drying technology .
The yarn strength has been improved to above 950MPa, the breathability has been improved to 600cm3/s, the dyeing uniformity has reached 99%, and the color fastness has reached 4-5 levels, which has reduced the defective rate and met the demand for high-quality yarns in the high-end market. , and reduce environmental pollution.
Smart Images

Figure CN118979318A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester yarn production technology, in particular to a production process for making polyester yarn from short fibers. Background Art
[0002] Polyester yarn usually refers to the cotton yarn used to produce polyester. Polyester is a type of fiber made from polymers through spinning. Currently, it is mainly produced from polyethylene terephthalate, commonly known as polyester in my country, or "PET" fiber for short. "Yarn" is a long and thin object with a certain strength and linear density formed by arranging many short fibers or filaments in a nearly parallel state and twisting them along the axial direction; while "thread" is a strand of yarn twisted together from two or more single yarns. Polyester staple fiber is a short fiber with a length of several centimeters to more than ten centimeters. It is obtained by spinning polyester (i.e. polyethylene terephthalate, which is polymerized from PTA and MEG) into a tow and cutting it.
[0003] There are many significant problems in the existing production process of polyester yarn made from staple fibers, especially in the blending process: first, the determination of the blending ratio lacks scientificity and accuracy, resulting in unstable yarn performance and failure to give full play to the advantages of different types of staple fibers; second, the blending method is mostly simple random mixing, without the orderly layered alternation method, resulting in uneven fiber distribution, different gap sizes, and poor yarn strength, wear resistance and anti-pilling performance; at the same time, the length and fineness of the staple fibers are not accurately classified, and the laying order is chaotic, resulting in loose fiber bonding, affecting the yarn quality, and it is difficult to solve the problem. To solve the problem of uneven fiber laying, thus increasing the defective rate; there is also improper selection of finishing agents, most of which are non-environmentally friendly, which is not only unfriendly to the environment, but also has poor treatment effects and cannot effectively improve the color fastness, antibacterial properties and softness of the yarn; in summary, the existing production process of polyester yarn made of short fibers has many defects in the blending process and post-processing links, and cannot produce high-quality polyester yarn with high strength, high air permeability, high dyeing uniformity, high color fastness and good softness, which is difficult to meet the market demand for high-end textiles. An innovative and optimized production process is urgently needed to solve these problems.
[0004] In view of this, a production process for making polyester yarn from short fibers is provided to overcome the above problems. Summary of the invention
[0005] The object of the present invention is to provide a production process for making polyester yarn from short fibers to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides a production process for preparing polyester yarn from short fibers, comprising the following steps:
[0007] S1. Fiber pretreatment: Classify and screen the short fibers to remove impurities and unqualified fibers; soak the screened short fibers in a reagent combination of 5% sodium hydroxide solution and 3% hydrogen peroxide solution in a ratio of 2:1 for 30 minutes;
[0008] S2, blending process:
[0009] S2.1, blending ratio: set to 40% of type A staple fiber and 60% of type B staple fiber;
[0010] S2.2, humidification: before blending, the two types of short fibers are pre-humidified to control the moisture content to 8%;
[0011] S2.3, layered alternating mixing: the blending method is to evenly lay a layer of type A staple fiber first, then lay a layer of type B staple fiber, and so on alternately;
[0012] S2.4, fine blending: Classify the length and fineness of type A and type B staple fibers: For type A staple fibers, they are divided into three categories according to their length: short, medium and long, and their fineness is also divided into three levels: fine, medium and coarse; type B staple fibers are classified in the same way; when laying the first layer of type A staple fibers, they are arranged in the order from fine to coarse, from short to long; then lay the first layer of type B staple fibers, also in the order from fine to coarse, from short to long, but at a 45-degree angle to the arrangement direction of type A staple fibers;
[0013] S2.5, Laying: Use automatic laying equipment; and use ultrasonic wave to assist blending, the frequency is set to 30kHz, and the action time is 20 minutes;
[0014] S3, spinning preparation: use spinning auxiliaries: including 5% silicone oil, 3% antistatic agent and 2% softener;
[0015] S4, spinning process: in the high-speed rotary air-jet spinning technology, the air velocity is set to 300 m / s, and the spinning twist is 1000 twists / m;
[0016] S5. Post-processing:
[0017] S5.1. Temperature control: The heat setting temperature is controlled at 180°C, the stretching ratio is 1.5 times, and the duration is 10 minutes;
[0018] S5.2, introduce environmentally friendly finishing agents, select tea tree extract and aloe vera extract, the concentration is 8%, soak for 20 minutes, control the pH value of the soaking liquid between 5.5-6.5, and control and adjust the temperature of the soaking liquid between 35℃-45℃;
[0019] S5.3, use ultraviolet irradiation, the intensity is 100W / m 2 , irradiation time 15 minutes;
[0020] S5.4. Use low-temperature vacuum drying, control the vacuum degree at -0.08MPa, the temperature at 50°C, and the drying time for 30 minutes.
[0021] Furthermore, in S1, the solution temperature was maintained at 40°C and stirred continuously during the immersion process; the fiber surface was treated with low-temperature plasma technology, and the discharge power was controlled to be 100 W, the treatment time was 10 minutes, and the gas flow rate was 10 L / min; then microwave radiation pretreatment was used, with a microwave frequency of 2450 MHz and a radiation time of 5 minutes, and a circulating water cooling system was used during the radiation process.
[0022] Furthermore, in S2.5, the fiber laying uniformity is monitored in real time. Through multiple high-definition cameras and image recognition technology installed on the automatic laying equipment, once an uneven area is found, the working parameters of the nozzle are automatically adjusted immediately.
[0023] Furthermore, in S2, a constant temperature and humidity environment is maintained in the blending room, with the temperature controlled at 25°C ± 2°C and the relative humidity controlled at 60% ± 5%.
[0024] Furthermore, in S3, when preparing the spinning aid, the silicone oil and the antistatic agent are first fully mixed, and then the softener is added and stirred evenly; the electrostatic field intensity is controlled at 50 kV / m, and the action time is 15 minutes.
[0025] Furthermore, in S4, a high-precision tension sensor is used to monitor the spinning tension in real time. The sensor is installed at the spinning spindle, the yarn guide wheel or the yarn guide rod, or in front of the yarn winding device.
[0026] Further, in S5.2, a circulating stirring device is used during the soaking process.
[0027] Furthermore, in S5.2, ultrasound-assisted penetration technology is introduced, with the ultrasound frequency set at 40 kHz and the action time being 10 minutes.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] Layered alternating mixing allows different types of short fibers to be more evenly distributed and interwoven; during the laying process, the fibers are arranged in a specific order and manner to ensure uniform gaps between the fibers, thus forming a more stable and uniform distribution in the yarn structure; this uniform structure helps to improve the strength of the yarn, enabling it to withstand greater tensile forces, reaching more than 950MPa; at the same time, the uniform fiber distribution also improves the air permeability of the yarn, increasing it to 600cm 3 / s or above; and, the uniform structure and good fiber bonding allow the dye to penetrate and adhere more evenly during dyeing, with a dyeing uniformity of more than 99% and a color fastness of 4-5 levels; high-quality yarns can be used to make more functional and comfortable textiles, such as high-performance sportswear, medical protective equipment, etc., which broadens the application range of the products and brings more market opportunities for enterprises.
[0030] By installing high-precision tension sensors at multiple locations such as the spinning spindle, the yarn guide wheel or the yarn guide rod, and in front of the yarn winding device, the tension changes during the spinning process can be fully and accurately monitored. When the tension exceeds the set threshold, the intelligent control system can automatically adjust quickly and accurately in a short time to ensure the stability of the tension of the yarn during the spinning process. Stable tension helps the orderly arrangement and close bonding of yarn fibers, thereby enhancing the strength of the yarn, making the yarn strength reach more than 900MPa, reducing the coefficient of variation of the elongation at break, and significantly reducing the defective rate. At the same time, stable tension can also reduce the defects of the yarn structure, improve the uniformity of the yarn, and then improve the air permeability, dyeing uniformity and color fastness, so that the various performance indicators of the yarn meet the requirements of the high-end market and enhance the competitiveness of the product.
[0031] Environmentally friendly finishing agents such as tea tree extract and aloe vera extract are selected, and their concentration, pH value, temperature and processing time are controlled. These natural extracts can form a protective film on the surface of the yarn, enhance the color fastness of the yarn to level 4-5, and are not easy to fade during use and washing. At the same time, the antibacterial inhibition rate is enhanced to more than 95%, and the softness is increased by more than 30%, further optimizing the performance of the yarn, meeting the high-end market's demanding needs for high-quality yarns, and enhancing the competitiveness of products in the market; the use of environmentally friendly finishing agents and low-temperature vacuum drying technologies reduces pollution to the environment, meets the current social requirements for sustainable development, and enhances the social image of the company. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a flow chart of a production process of polyester yarn made from short fibers. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] See also Figure 1 , the present invention provides a technical solution:
[0035] See also Figure 1 As shown, a production process of short fibers into polyester yarn comprises the following steps:
[0036] S1. Fiber pretreatment: Classify and screen the short fibers to remove impurities and unqualified fibers; soak the screened short fibers in a reagent combination of 5% sodium hydroxide solution and 3% hydrogen peroxide solution in a ratio of 2:1 for 30 minutes; keep the solution temperature at 40°C and stir continuously during the soaking process; and treat the fiber surface with low-temperature plasma technology, and control the discharge power to 100W, the treatment time to 10 minutes, and the gas flow rate to 10L / min; then use microwave radiation pretreatment, the frequency of microwaves is 2450MHz, the radiation time is 5 minutes, and a circulating water cooling system is used during the radiation process to prevent the fiber from overheating;
[0037] Specific implementation method:
[0038] Fiber classification and screening: You can use a vibrating screening machine to set the appropriate screen aperture and vibration frequency according to the fiber length, fineness and other parameters to remove impurities and unqualified fibers;
[0039] Soaking treatment: It is carried out in a soaking tank equipped with a heating and stirring device; first, a mixture of 5% sodium hydroxide solution and 3% hydrogen peroxide solution is prepared in proportion, and the screened short fibers are placed in the soaking tank. The solution temperature is maintained at 40°C by a temperature sensor and a heating element, and an electric stirrer is used to stir continuously;
[0040] Low-temperature plasma treatment: Use special low-temperature plasma treatment equipment, set the discharge power to 100W, the treatment time to 10 minutes, and the gas flow rate to 10L / min;
[0041] Microwave radiation pretreatment: Use industrial microwave radiation equipment, set the frequency to 2450MHz, irradiation time to 5 minutes, and start the circulating water cooling system at the same time;
[0042] Example 1 of fiber pretreatment:
[0043] Fiber classification and screening: Using a multi-layer screen with a pore size of 0.5-5 mm and a vibration frequency of 500 times / minute, 97% of impurities and unqualified fibers were successfully removed;
[0044] Soaking treatment: The stirring speed is 80 rpm, and the cleanliness of the fiber is increased by 90% after soaking;
[0045] Low-temperature plasma treatment: The surface roughness of the treated fiber is reduced and the hydrophilicity is improved;
[0046] Microwave radiation pretreatment: The crystallinity of the fiber is improved, and the subsequent spinning performance is improved;
[0047] The final polyester yarn has excellent performance in strength, abrasion resistance and anti-pilling performance; compared with the traditional pretreatment process, the strength is increased by 18%, the abrasion resistance is increased by 15%, and the anti-pilling grade is improved from level 2 to level 3.5;
[0048] Example 2 of fiber pretreatment:
[0049] Fiber classification and screening: The intelligent optical detection system is introduced to assist screening, and the impurity removal rate reaches 98%;
[0050] Soaking treatment: Use more precise temperature control and stirring device to achieve better soaking effect;
[0051] Low-temperature plasma treatment: optimize gas composition and further improve fiber surface properties;
[0052] Microwave radiation pretreatment: adjust the microwave radiation power to make the internal structure of the fiber more uniform;
[0053] The strength of the polyester yarn produced is 22% higher than that of the traditional process, the wear resistance is increased by 20%, and the anti-pilling grade reaches level 4;
[0054] Comparative Example 1 of Fiber Pretreatment:
[0055] Only simple manual sorting and screening is performed, and the impurity removal rate is about 70%;
[0056] No immersion, low-temperature plasma and microwave radiation treatments were performed;
[0057] The final properties of polyester yarn are similar to those of the traditional process, with no significant improvement;
[0058] Comparative Example 2 of Fiber Pretreatment:
[0059] The fiber classification screening and soaking treatment were carried out, but the soaking temperature was 30°C and the stirring speed was 50 rpm;
[0060] No low-temperature plasma and microwave radiation treatment was performed;
[0061] The strength of the polyester yarn produced by the traditional process is 8% higher, the wear resistance is 5% higher, and the anti-pilling grade is 2.5;
[0062] Comparative Example 3 of Fiber Pretreatment:
[0063] The fiber is classified and screened, soaked and treated with low-temperature plasma. The discharge power of the low-temperature plasma treatment is 80W and the treatment time is 5 minutes.
[0064] Omit microwave radiation pretreatment;
[0065] The strength of the resulting polyester yarn is 12% higher than that of the traditional process, the abrasion resistance is increased by 8%, and the anti-pilling grade is level 3;
[0066] The following conclusions can be drawn from the above fiber pretreatment examples and comparative data:
[0067] The optimal method includes: 5% sodium hydroxide solution and 3% hydrogen peroxide solution mixed in a ratio of 2:1, immersion temperature of 40°C, stirring speed of more than 80 rpm, low-temperature plasma discharge power of 100W, treatment time of 10 minutes, gas flow rate of 10L / min and 2450MHz microwave radiation for 5 minutes;
[0068] The effects of fiber pretreatment are:
[0069] Greatly improve the strength of polyester yarn, so that it can withstand greater stretching and wear, suitable for making high-strength textiles, such as industrial fabrics; significantly enhance wear resistance, extend the service life of textiles, and reduce replacement costs; effectively improve anti-pilling performance, enhance product appearance quality and comfort, and meet consumer demand for high-quality textiles; optimize the surface and internal structure of the fiber, provide a good foundation for subsequent blending, spinning and post-processing processes, and improve the efficiency of the entire production process and the stability of product quality;
[0070] S2, blending process:
[0071] S2.1, blending ratio: set to 40% of type A staple fiber and 60% of type B staple fiber;
[0072] S2.2, humidification: before blending, the two types of short fibers are pre-humidified to control the moisture content to 8%;
[0073] S2.3, layered alternating mixing: the blending method is to evenly lay a layer of type A staple fiber first, then lay a layer of type B staple fiber, and so on alternately;
[0074] S2.4, fine blending: Classify the length and fineness of type A and type B staple fibers: For type A staple fibers, they are divided into three categories according to their length: short, medium and long, and their fineness is also divided into three levels: fine, medium and coarse; type B staple fibers are classified in the same way; when laying the first layer of type A staple fibers, they are arranged in the order from fine to coarse, from short to long; then lay the first layer of type B staple fibers, also in the order from fine to coarse, from short to long, but at a 45-degree angle to the arrangement direction of type A staple fibers;
[0075] S2.5, Laying: Use automatic laying equipment; monitor the laying uniformity of the fibers in real time, and automatically adjust the working parameters of the nozzles once an uneven area is found through multiple high-definition cameras and image recognition technology installed on the automatic laying equipment; and use ultrasonic waves to assist blending, with the frequency set to 30kHz and the action time set to 20 minutes; maintain a constant temperature and humidity environment in the blending room, with the temperature controlled at 25℃±2℃ and the relative humidity controlled at 60%±5%, to reduce the generation of static electricity and moisture absorption differences of the fibers during the laying process, and further ensure the uniformity and stability of the blending;
[0076] Example description:
[0077] Embodiment 1 of blending process:
[0078] Using a high-precision metering device, 40 kg of type A staple fibers and 60 kg of type B staple fibers were accurately weighed. The actual blending ratio was 40.5% type A and 59.5% type B.
[0079] The short fibers were pre-humidified by a spray humidifier to control the moisture content to 8.5%;
[0080] Using advanced automatic laying equipment, first lay a layer of type A short fiber evenly, then lay a layer of type B short fiber, alternately operate, and the laying effect is uniform;
[0081] Use professional fiber measuring equipment to classify type A and type B staple fibers. When laying the first layer of type A staple fibers, strictly follow the order from thin to thick and from short to long. When laying the first layer of type B staple fibers, the arrangement direction is 45 degrees to that of type A staple fibers.
[0082] Eight high-definition cameras and an advanced image recognition system are installed on the automatic laying equipment to monitor the uniformity of fiber laying in real time. Once an uneven area is found, the nozzle working parameters are automatically adjusted within 0.1 seconds. Ultrasonic waves assist blending at a frequency of 30kHz for 20 minutes, and the temperature in the blending chamber is stabilized at 23°C and the relative humidity is 58%.
[0083] The final polyester yarn has excellent performance in strength, abrasion resistance and anti-pilling performance. Compared with the polyester yarn produced by conventional blending process, the strength is increased by 20%, the abrasion resistance is increased by 18%, and the anti-pilling performance is improved from level 3 to level 4.
[0084] Embodiment 2 of blending process:
[0085] With the help of an automated fiber delivery system, the fibers are delivered in a ratio of 40% type A staple fibers and 60% type B staple fibers. The actual ratio is 39.2% type A and 60.8% type B.
[0086] Use steam pre-humidification to make the moisture content of short fibers reach 7.8%;
[0087] Using intelligent automatic laying equipment, the alternating laying process is smooth and without obvious defects;
[0088] High-precision laser measurement technology is used to sort and lay the fibers in the correct order;
[0089] The image recognition technology and nozzle adjustment system response time is 0.08 seconds, the ultrasonic-assisted blending effect is significant, and the blending room temperature is maintained at 27°C and the relative humidity is 62%;
[0090] The strength of the polyester yarn produced has increased by 22%, the abrasion resistance has increased by 20%, and the anti-pilling performance has reached level 4.5;
[0091] Comparative Example 1 of Blending Process:
[0092] The blending ratio is 20% of type A staple fiber and 80% of type B staple fiber;
[0093] No pre-humidification treatment is performed;
[0094] Randomly mix two types of short fibers without alternating layers;
[0095] Short fibers are not sorted by length and fineness and are laid randomly;
[0096] The fiber laying uniformity was manually observed, there was no automatic nozzle adjustment function, no ultrasonic assisted blending was used, the blending room temperature was 30°C, and the relative humidity was 45%;
[0097] The strength, abrasion resistance and anti-pilling performance of the produced polyester yarn are significantly lower than those of the embodiment. The strength is only 70% of that of the embodiment 1 of the blending process, the abrasion resistance is reduced by 30%, and the anti-pilling performance is level 2;
[0098] Comparative Example 2 of Blending Process:
[0099] The blending ratio is 50% type A staple fiber and 50% type B staple fiber;
[0100] Pre-humidification treatment but the moisture content is controlled at 5%;
[0101] The layers are mixed alternately but laid unevenly;
[0102] Inaccurate classification of short fibers and wrong laying order;
[0103] There is image recognition but the nozzle is not adjusted in time, the ultrasonic frequency is 20kHz, the temperature of the blending room is 20℃, and the relative humidity is 50%;
[0104] The performance of the polyester yarn produced in this comparative example is also inferior to that of the example, with a strength of 85% of that of the example 1 in the blending process, abrasion resistance reduced by 20%, and anti-pilling performance of level 3;
[0105] Through the above blending process embodiment and comparative example data, the following conclusions can be drawn:
[0106] The optimal method includes: accurate blending ratio (40% for type A and 60% for type B), proper pre-humidification treatment (moisture content of about 8%), alternating layered blending, precise fiber classification and laying sequence, efficient automatic laying and monitoring and adjustment equipment, appropriate ultrasonic-assisted blending, and a stable constant temperature and humidity environment;
[0107] The effect is:
[0108] Significantly improve the strength of polyester yarn, making it more durable and less likely to break in subsequent textile applications; enhance wear resistance, extend product life, and reduce replacement costs; improve anti-pilling performance, enhance product appearance quality and comfort, and meet consumers' high-quality needs; ensure the uniformity and stability of blending, improve product quality consistency, and reduce defective rates;
[0109] S3, spinning preparation: use spinning auxiliaries: including 5% silicone oil, 3% antistatic agent and 2% softener; when preparing spinning auxiliaries, first mix the silicone oil and antistatic agent thoroughly, then add the softener and stir evenly; the electrostatic field intensity is controlled at 50kV / m, and the action time is 15 minutes;
[0110] Spinning preparation embodiment 1:
[0111] Spinning auxiliaries preparation: accurately weigh 50g silicone oil, 30g antistatic agent and 20g softener; first stir the silicone oil and antistatic agent in a stirrer at 300 rpm for 10 minutes to fully mix them; then add the softener and continue stirring for 5 minutes until the mixture is evenly mixed;
[0112] Electrostatic field treatment: In a special electrostatic treatment device, set the electrostatic field strength to 50kV / m and let the fiber act in the electric field for 15 minutes;
[0113] After this spinning preparation process, the polyester yarn produced has excellent softness, antistatic performance and smoothness; compared with the conventional spinning preparation process, the softness is improved by 20%, the antistatic performance is reduced from the surface resistance of 10^10 ohms to 10^8 ohms, and the smoothness is also significantly improved;
[0114] Embodiment 2 of spinning preparation:
[0115] Spinning auxiliaries configuration: Use high-precision measuring instruments to weigh 55 grams of silicone oil, 25 grams of antistatic agent and 20 grams of softener; first stir the silicone oil and antistatic agent in a sealed stirring container at 400 rpm for 8 minutes, add the softener after fully mixing, and stir for another 6 minutes to ensure uniformity;
[0116] Electrostatic field treatment: Optimize the parameters of electrostatic treatment equipment to stabilize the electrostatic field intensity at 52kV / m, and strictly control the fiber action time at 15 minutes;
[0117] The resulting polyester yarn has a further 25% softness increase, antistatic properties reach a surface resistance of 10^7 ohms, and smoothness is significantly enhanced;
[0118] Comparative Example 1 of Spinning Preparation:
[0119] Spinning auxiliaries configuration: only 3% silicone oil, 2% antistatic agent and 1% softener are used, and the stirring is not sufficient;
[0120] Electrostatic field treatment: Electrostatic field intensity is 30kV / m, action time is 10 minutes;
[0121] The polyester yarn produced in this comparative example has poor softness, antistatic performance and smoothness. Compared with the spinning preparation in Example 1, the softness is reduced by 30%, the antistatic performance is a surface resistance of 10^11 ohms, and the smoothness is also obviously insufficient.
[0122] Comparative Example 2 of Spinning Preparation:
[0123] Spinning auxiliaries configuration: 8% silicone oil, 1% antistatic agent and 1% softener are used, and the stirring order is wrong;
[0124] Electrostatic field treatment: The electrostatic field intensity is unstable, fluctuating between 40-60 kV / m, and the action time is 18 minutes;
[0125] The properties of the produced polyester yarn are uneven, with too high softness but insufficient antistatic properties, and the smoothness is not as good as the spinning preparation embodiment;
[0126] Through the above spinning preparation examples and comparative data, the following conclusions can be drawn:
[0127] The optimal composition includes 5% silicone oil, 3% antistatic agent and 2% softener; the method is to first fully mix the silicone oil and antistatic agent, then add the softener and stir evenly, while the electrostatic field intensity is controlled at 50kV / m, and the action time is 15 minutes;
[0128] The effect is:
[0129] Significantly improve the softness of polyester yarn, so that it has better feel and comfort in subsequent textile processing and use, and is suitable for making underwear, etc.; effectively enhance antistatic performance, reduce static electricity accumulation in yarn during processing and use, improve production efficiency and product quality, and avoid the adverse effects of static electricity on products; improve the smoothness of yarn, reduce the friction coefficient, which is beneficial to subsequent textile processes, reduce the occurrence of broken ends and defects, and improve the continuity and stability of production;
[0130] S4. Spinning process: In high-speed rotary air spinning technology, the air flow speed is set to 300m / s and the spinning twist is 1000 twists / m; a high-precision tension sensor is used to monitor the spinning tension in real time. The sensor is installed at the spinning spindle, the yarn guide wheel or the yarn guide rod, and in front of the yarn winding device to ensure accurate measurement of the tension; when the tension exceeds the set threshold, it is automatically adjusted within 0.5 seconds through the intelligent control system. The algorithm of the intelligent control system should be optimized to achieve fast and accurate adjustment;
[0131] Embodiment 1 of spinning process:
[0132] Air flow speed: Use precise air flow control equipment to stably set the air flow speed to 300m / s;
[0133] Spinning twist: Through advanced spinning equipment, the spinning twist is accurately controlled to 1000 twists / m;
[0134] Tension monitoring and adjustment: High-precision tension sensors are installed at the spinning spindles, yarn guide wheels and yarn guide rods, and in front of the yarn winding device; when the tension exceeds the set threshold (e.g. 10N), the intelligent control system quickly makes adjustments within 0.5 seconds, with an adjustment accuracy of ±0.5N;
[0135] The polyester yarn produced by this spinning process has good strength uniformity and the coefficient of variation of elongation at break is as low as 5%. Compared with the traditional spinning process, the quality stability of the yarn is greatly improved and the defective rate is reduced by 20%.
[0136] Embodiment 2 of spinning process:
[0137] Air flow speed: Further optimize air flow control to control the air flow speed fluctuation range within ±5m / s and the average speed is 300m / s;
[0138] Spinning twist: Use a more precise spinning twist control device to control the spinning twist deviation within ±5 twists / m, and the actual average twist is 1000 twists / m;
[0139] Tension monitoring and adjustment: Increase the number and accuracy of tension sensors, set the tension threshold to 8N, shorten the adjustment time of the intelligent control system to 0.4 seconds, and achieve an adjustment accuracy of ±0.3N;
[0140] The obtained polyester yarn has excellent strength uniformity, and the coefficient of variation of elongation at break is only 3%. The product quality is significantly better than that of Example 1 of the spinning process, and the defective rate is further reduced to 5%;
[0141] Comparative Example 1 of Spinning Process:
[0142] Air flow speed: The air flow speed is unstable, fluctuating between 250-350m / s; Spinning twist: The spinning twist control is inaccurate, varying between 800-1200 twists / m; Tension monitoring and adjustment: The tension sensor is only installed at the spinning spindle, the tension threshold is not set properly (for example, 15N), the adjustment time is as long as 2 seconds, and the adjustment accuracy is ±2N;
[0143] The polyester yarn produced under this condition has poor strength uniformity, a coefficient of variation of elongation at break as high as 15%, and a defective rate as high as 30%;
[0144] Comparative Example 2 of Spinning Process:
[0145] Air flow speed: the air flow speed is set to 280m / s; Spinning twist: the spinning twist is 800 twists / m; Tension monitoring and adjustment: a tension sensor with lower accuracy is installed at the yarn guide wheel, the tension threshold is 12N, the adjustment time is 1 second, and the adjustment accuracy is ±1.5N; The quality of the obtained polyester yarn is obviously inferior to that of the embodiment, the coefficient of variation of the elongation at break is 10%, and the defective rate is 20%;
[0146] Through the above spinning process embodiments and comparative example data, the following conclusions can be drawn:
[0147] The optimal method includes: stable air flow speed of 300m / s, accurate spinning twist of 1000 twists / m, comprehensive and high-precision tension monitoring (sensors are installed at the spinning spindle, yarn guide wheel or yarn guide rod, and in front of the yarn winding device), and fast and accurate (within 0.5 seconds, accuracy ±0.5N) tension adjustment intelligent control system;
[0148] The effect is:
[0149] Significantly improve the quality stability of polyester yarn, ensure that the yarn has a high degree of consistency in strength, elongation, etc., and meet the strict requirements of high-end textiles on yarn quality; significantly reduce the defective rate, reduce the waste of raw materials, and improve production efficiency and economic benefits; precise tension control helps to reduce the phenomenon of yarn breakage during the spinning process and improve production continuity and efficiency; stable and appropriate air flow speed and spinning twist can optimize the structure and performance of the yarn, making it have better physical properties and textile processing performance;
[0150] S5. Post-processing:
[0151] S5.1. Temperature control: The heat setting temperature is controlled at 180°C, the stretching ratio is 1.5 times, and the duration is 10 minutes;
[0152] S5.2, introduce environmentally friendly finishing agents, select tea tree extract and aloe vera extract, the concentration is 8%, soak for 20 minutes, control the pH value of the soaking liquid between 5.5-6.5, and control and adjust the temperature of the soaking liquid between 35℃-45℃; use a circulating stirring device during the soaking process to ensure that the yarn is fully in contact with the finishing agent, and also introduce ultrasonic assisted penetration technology, the ultrasonic frequency is set at 40kHz, the action time is 10 minutes, to accelerate the penetration and uniform distribution of the finishing agent inside the yarn;
[0153] S5.3, use ultraviolet irradiation, the intensity is 100W / m 2 , irradiation time 15 minutes;
[0154] S5.4, low temperature vacuum drying is adopted, the vacuum degree is controlled at -0.08MPa, the temperature is 50℃, and the drying time is 30 minutes;
[0155] Example 1 of post-processing:
[0156] During the heat setting process, precise temperature control equipment is used to stably control the temperature at 180°C, the stretching multiple is accurately set to 1.5 times, and the duration is strictly controlled to 10 minutes; high-quality tea tree extract and aloe vera extract are selected as environmentally friendly finishing agents, and the concentration is accurately configured to 8%; the pH value of the soaking liquid is controlled at 6.0 and the temperature is maintained at 40°C; the circulating stirring device runs at a speed of 80 rpm, the ultrasonic frequency is 40kHz, and the action time is 10 minutes; the ultraviolet irradiation intensity is stabilized at 100W / m 2 , the irradiation time is precisely controlled to be 15 minutes; during low-temperature vacuum drying, the vacuum degree is precisely controlled at -0.08MPa, the temperature is maintained at 50°C, and the drying time is 30 minutes;
[0157] After this post-treatment process, the polyester yarn produced has excellent performance in color fastness, antibacterial properties and softness; compared with the conventional post-treatment process, the color fastness is improved by 2 levels, the inhibition rate of antibacterial properties against common bacteria reaches more than 95%, and the softness is improved by 30%;
[0158] Example 2 of post-processing:
[0159] The heat setting temperature control accuracy reaches ±1℃, the stretching multiple deviation is less than 0.1 times, and the duration error does not exceed 1 minute;
[0160] Strictly control the quality and concentration of the finishing agent, the pH value of the soaking solution is 5.8 and the temperature is 38°C;
[0161] The circulating stirring speed is increased to 100 rpm, and the ultrasonic effect is better;
[0162] The UV radiation intensity fluctuation range is ±5W / m 2 The irradiation time is controlled precisely; the vacuum degree is controlled more accurately, the temperature fluctuation is less than ±2℃, and the drying time is accurate;
[0163] The color fastness of the obtained polyester yarn is further improved to level 4-5, the antibacterial property has an inhibition rate of 98% against common bacteria, and the softness is improved by 35%;
[0164] Comparative Example 1 of Post-treatment:
[0165] The heat setting temperature is 160°C, the stretching ratio is 1.2 times, and the duration is 8 minutes;
[0166] The concentration of finishing agent was 5%, the pH value of soaking solution was 5.0, the temperature was 30°C, the circulation stirring speed was 50 rpm, and there was no ultrasonic assistance;
[0167] The UV radiation intensity is 80W / m 2 , irradiation time is 10 minutes; vacuum degree is -0.06MPa, temperature is 40℃, and drying time is 20 minutes;
[0168] The polyester yarn produced in this comparative ratio is obviously inferior in color fastness, antibacterial performance and softness, with color fastness of 2-3, antibacterial inhibition rate of about 70%, and softness improvement of less than 10%;
[0169] Comparative Example 2 of Post-treatment:
[0170] The heat setting temperature is 200°C, the stretching ratio is 2.0 times, and the duration is 12 minutes;
[0171] The concentration of the finishing agent was 10%, the pH value of the soaking solution was 7.0, the temperature was 50°C, the circulating stirring speed was 120 rpm, and the ultrasonic frequency was too high;
[0172] The UV radiation intensity is 120W / m 2 , irradiation time is 20 minutes; vacuum degree is -0.1MPa, temperature is 60℃, and drying time is 40 minutes;
[0173] The performance of the polyester yarn in this comparative example is uneven, with some properties improved, but the overall quality is not as good as that of the embodiment, and there is fiber damage caused by over-treatment;
[0174] Through the above post-processing examples and comparative data, the following conclusions can be drawn:
[0175] The optimal method includes: heat setting temperature of 180℃, stretching ratio of 1.5 times, duration of 10 minutes; finishing agent concentration of 8%, soaking liquid pH value of 5.5-6.5, temperature of 35-45℃, circulating stirring and 40kHz ultrasonic assistance for 10 minutes;
[0176] UV radiation intensity 100W / m 2 , irradiation time 15 minutes; vacuum degree of low temperature vacuum drying -0.08MPa, temperature 50℃, drying time 30 minutes;
[0177] The effect is:
[0178] Significantly improve the color fastness of polyester yarn, making it less likely to fade during use and washing, maintaining bright colors, and improving the appearance quality and durability of the product; enhance antibacterial properties, so that textiles made of polyester yarn have better hygiene and health functions, meeting consumers' health needs; effectively improve softness, increase the comfort and touch of textiles, and improve the market competitiveness of products; the optimized post-processing process can ensure the stability and consistency of yarn performance, improve production efficiency and product qualification rate.
[0179] Summarize:
[0180] This production process includes five steps: fiber pretreatment, blending process, spinning preparation, spinning process and post-treatment. Fiber pretreatment optimizes fibers through operations such as classification and screening, soaking in specific reagents, etc.; the blending process sets the proportion, pre-humidification, layered alternating blending, etc. to improve the blending effect; the spinning preparation determines the auxiliary agent components and electrostatic field treatment parameters; the spinning process controls the air flow speed, spinning twist and tension monitoring and adjustment; post-treatment includes heat setting, environmentally friendly finishing agent treatment, etc. Each step has an example, a comparative example and the conclusion of the optimal method, and all have significant effects.
[0181] Layered alternating mixing method in the blending process:
[0182]
[0183] Layered alternating mixing allows different types of short fibers to be more evenly distributed and interwoven; during the laying process, the fibers are arranged in a specific order and manner to ensure uniform gaps between the fibers, thus forming a more stable and uniform distribution in the yarn structure; this uniform structure helps to improve the strength of the yarn, enabling it to withstand greater tensile forces, reaching more than 950MPa; at the same time, the uniform fiber distribution also improves the air permeability of the yarn, increasing it to 600cm 3 / s or above; and, the uniform structure and good fiber bonding allow the dye to penetrate and adhere more evenly during dyeing, with a dyeing uniformity of more than 99% and a color fastness of 4-5 levels; high-quality yarns can be used to make more functional and comfortable textiles, such as high-performance sportswear, medical protective equipment, etc., which broadens the application range of the products and brings more market opportunities for enterprises.
[0184] Real-time tension monitoring and automatic adjustment during spinning:
[0185]
[0186] By installing high-precision tension sensors at multiple locations such as the spinning spindle, the yarn guide wheel or the yarn guide rod, and in front of the yarn winding device, the tension changes during the spinning process can be fully and accurately monitored. When the tension exceeds the set threshold, the intelligent control system can automatically adjust quickly and accurately in a short time (within 0.5 seconds), ensuring the stability of the tension of the yarn during the spinning process. Stable tension helps the orderly arrangement and close bonding of yarn fibers, thereby enhancing the strength of the yarn, making the yarn strength reach more than 900MPa, reducing the coefficient of variation of the elongation at break, and significantly reducing the defective rate. At the same time, stable tension can also reduce the defects of the yarn structure, improve the uniformity of the yarn, and then improve the air permeability, dyeing uniformity and color fastness, so that the various performance indicators of the yarn meet the requirements of the high-end market and enhance the competitiveness of the product.
[0187] Selection of environmentally friendly finishing agents in post-processing steps:
[0188]
[0189] Environmentally friendly finishing agents such as tea tree extract and aloe vera extract are selected, and their concentration, pH value, temperature and processing time are controlled. These natural extracts can form a protective film on the surface of the yarn, enhance the color fastness of the yarn to level 4-5, and are not easy to fade during use and washing. At the same time, the antibacterial inhibition rate is enhanced to more than 95%, and the softness is increased by more than 30%, further optimizing the performance of the yarn, meeting the high-end market's demanding needs for high-quality yarns, and enhancing the competitiveness of products in the market; the use of environmentally friendly finishing agents and low-temperature vacuum drying technologies reduces pollution to the environment, meets the current social requirements for sustainable development, and enhances the social image of the company.
Claims
1. A production process for producing polyester yarn from short fibers, characterized in that: The following steps are involved: S1. Fiber pretreatment: Classify and screen short fibers to remove impurities and unqualified fibers; The screened short fibers are immersed in a reagent combination of a 5% sodium hydroxide solution and a 3% hydrogen peroxide solution in a ratio of 2:1, and the short fibers are immersed for 30 minutes; S2, blending process: S2.1, blending ratio: set to 40% of type A staple fiber and 60% of type B staple fiber; S2.2, humidification: before blending, the two types of short fibers are pre-humidified to control the moisture content to 8%; S2.3, layered alternating mixing: the blending method is to evenly lay a layer of type A staple fiber first, then lay a layer of type B staple fiber, and so on alternately; S2.4, fine blending: Classify the length and fineness of type A and type B staple fibers: For type A staple fibers, they are divided into three categories according to their length: short, medium and long, and their fineness is also divided into three levels: fine, medium and coarse; type B staple fibers are classified in the same way; when laying the first layer of type A staple fibers, they are arranged in the order from fine to coarse, from short to long; then lay the first layer of type B staple fibers, also in the order from fine to coarse, from short to long, but at a 45-degree angle to the arrangement direction of type A staple fibers; S2.5, Laying: Use automatic laying equipment; and use ultrasonic wave to assist blending, the frequency is set to 30kHz, and the action time is 20 minutes; S3, spinning preparation: use spinning auxiliaries: including 5% silicone oil, 3% antistatic agent and 2% softener; S4, spinning process: in the high-speed rotary air-jet spinning technology, the air velocity is set to 300 m / s, and the spinning twist is 1000 twists / m; S5. Post-processing: S5.
1. Temperature control: The heat setting temperature is controlled at 180°C, the stretching ratio is 1.5 times, and the duration is 10 minutes; S5.2, introduce environmentally friendly finishing agents, select tea tree extract and aloe vera extract, the concentration is 8%, soak for 20 minutes, control the pH value of the soaking liquid between 5.5-6.5, and control and adjust the temperature of the soaking liquid between 35℃-45℃; S5.3, use ultraviolet irradiation, the intensity is 100W / m 2 , irradiation time 15 minutes; S5.
4. Use low-temperature vacuum drying, control the vacuum degree at -0.08MPa, the temperature at 50°C, and the drying time for 30 minutes.
2. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S1, the solution temperature was maintained at 40°C during the immersion process and was continuously stirred; the fiber surface was treated with low-temperature plasma technology, and the discharge power was controlled to be 100 W, the treatment time was 10 minutes, and the gas flow rate was 10 L / min; then microwave radiation pretreatment was used, with a microwave frequency of 2450 MHz and a radiation time of 5 minutes. A circulating water cooling system was used during the radiation process.
3. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S2.5, the fiber laying uniformity is monitored in real time. Through multiple high-definition cameras and image recognition technology installed on the automatic laying equipment, once an uneven area is found, the working parameters of the nozzle are automatically adjusted immediately.
4. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S2, a constant temperature and humidity environment is maintained in the blending room, with the temperature controlled at 25°C ± 2°C and the relative humidity controlled at 60% ± 5%.
5. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S3, when preparing the spinning auxiliaries, first mix the silicone oil and the antistatic agent thoroughly, then add the softener and stir evenly; the electrostatic field intensity is controlled at 50 kV / m, and the action time is 15 minutes.
6. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S4, a high-precision tension sensor is used to monitor the spinning tension in real time. The sensor is installed at the spinning spindle, the yarn guide wheel or the yarn guide rod, and in front of the yarn winding device.
7. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S5.2, a circulating agitation device is used during the soaking process.
8. The process for producing polyester yarn from staple fibers as claimed in claim 1, characterized in that: In S5.2, ultrasound-assisted penetration technology is also introduced, with the ultrasound frequency set at 40kHz and the action time being 10 minutes.
Citation Information
Patent Citations
Green dyeing-finishing processing technology for textiles
CN104631158A
Preparation method of long-acting anti-microbial textile
CN106978721A
Graphene biologic diatom compound fiber and preparation method and application thereof
CN108374218A
Pretreatment process before yarn dyeing
CN109750505A
Production method of combed blended yarn
CN110004544A