Blended broken filament interwoven antistatic clothing fabric and manufacturing method thereof

By employing specific processing techniques for blended wool and silk fabrics, the shortcomings of worsted wool antistatic fabrics in point-to-point resistance testing have been overcome, achieving highly efficient antistatic performance and making them suitable for flammable, explosive, and high-risk environments.

CN118979326APending Publication Date: 2024-11-19SHANDONG NANSHAN TEXTILE GARMENT
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411141636.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing worsted wool antistatic fabrics are insufficient in terms of antistatic effect and point-to-point resistance testing, making it difficult to meet the high antistatic requirements of flammable, explosive, and high-risk production, storage, and transportation units.

Method used

It adopts a blended structure of 64S Australian wool, 2D polyester fiber, mulberry silk, Tencel and 20D nylon matrix conductive filaments, combined with specific spinning, weaving and dyeing and finishing processes, including B412 blending, recombing, warping, weaving, singeing, continuous boiling, washing and drying, to ensure the reasonable distribution of conductive filaments and fabric quality.

Benefits of technology

It can pass both static charge tests and point-to-point resistance tests, meeting the safety requirements of high-risk environments such as oil fields, gas stations, and flour mills, and providing more efficient antistatic performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of wool worsted fabric application, and particularly discloses a blended broken filament interwoven antistatic clothing fabric and a manufacturing method thereof. The method is used for solving the problem that the conventional wool worsted antistatic fabric cannot meet the point-to-point resistance test requirement. The blended broken filament interwoven antistatic clothing fabric is prepared from the following raw materials in percentage by weight: 50% of 64S Australasian wool, 39.6% of 2D polyester fibers, 5% of mulberry silk, 5% of tencel and 0.4% of 20D chinlon matrix conductive filaments. The texture is 1 / 1 plain weave; the gram weight is 230 g, and the yarn count is 78 / 2 * 78 / 2 metric count; and the warp and weft density is 288 * 260 pieces / 10cm. The manufacturing method comprises a spinning process, a weaving process and a dyeing and finishing process. The comprehensive content of the conductive filaments is 0.4%, but the conductivity of the conductive filaments exceeds that of a fabric mixed with 5% of common conductive short fibers. The device can pass an electrostatic charge test and a point-to-point resistance test, and meets the safety requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wool worsted fabric application, and in particular relates to a blended wool and silk interwoven antistatic clothing fabric and a manufacturing method thereof. Background Art

[0002] Conventional wool worsted antistatic fabrics have certain antistatic properties by adding conductive fibers, but their conductivity is poor. In order to meet the high antistatic requirements of flammable and explosive high-risk production, storage and transportation units such as oil fields, gas stations, flour mills, and oil presses, it is necessary to develop a type of wool blended high-efficiency antistatic clothing fabric that can meet both static charge indicators and point-to-point conductivity indicators.

[0003] In the current market, most wool-blended antistatic fabrics contain a small amount of conductive fiber (short fiber type). Conductive fiber is generally a polyester matrix or a nylon matrix. In actual use, an appropriate amount of conductive fiber is added according to market needs. However, this type of antistatic fabric has major problems: first, the antistatic effect is not ideal; second, although it can meet the requirements of the static charge test, it cannot meet the requirements of the point-to-point resistance test.

[0004] Therefore, it is of great significance to provide an antistatic clothing fabric that can meet both the requirements of electrostatic charge test and the requirements of point-to-point resistance test. Summary of the invention

[0005] One object of the present invention is to provide a blended wool-silk antistatic clothing fabric, which effectively solves the problem that conventional wool worsted antistatic fabrics cannot meet the requirements of point-to-point resistance testing.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a blended wool-silk interwoven antistatic clothing fabric, the raw materials and the comprehensive proportion of the raw materials used are: 64S Australian wool 50%, 2D polyester fiber 39.6%, mulberry silk 5%, Tencel 5% and 20D nylon matrix conductive filament 0.4%. The organization is 1 / 1 plain weave; the gram weight is 230g, the yarn count is 78 / 2*78 / 2 public count; the warp and weft density is 288*260 strands / 10cm.

[0007] Another object of the present invention is to provide a method for making the blended wool-silk interwoven antistatic clothing fabric described in the above embodiments, including a spinning process, a weaving process and a dyeing and finishing process, wherein the spinning process includes B412 blending, three needle combings before re-combing, re-combing, two needles after re-combing, four needle combings before spinning, roving, spun yarn, one-time steaming, winding, paralleling, doubling and two-time steaming, the weaving process includes warping, drawing-in, weaving and grey cloth, and the dyeing and finishing process includes singeing, one-time continuous boiling, rope-shaped washing, opening width, two-time continuous boiling, drying, center inspection, trimming, shearing, moistening, calendering, tank steaming and finished product.

[0008] Furthermore, in the spinning process, the warp D yarn and the weft B yarn are spun at 44 Nm / 1, twist direction Z, and twist degree 600 T / m; the B yarn is 20D nylon matrix conductive filament; the A yarn and the B yarn are spun together to form 78 Nm / 2 yarn, twist direction S, and twist degree 1050 T / m.

[0009] Furthermore, in the weaving process, warping is performed using a warping machine, the tension of the single yarn is controlled at 18CN, cold sizing is added in the reversing process, the sizing amount is 40, and the reversing speed is <90m / min.

[0010] Drawing-in, reed drawing-in and drop wire drawing are done using Swiss Stäubli equipment, and the three operations are completed at one time with a machine speed of 260 yarns / min.

[0011] During weaving, the warp yarn arrangement is 10A.1D.4B.[1C].11A.4B1C.2A.1D.8A.4B1C / 48, and the weft yarn arrangement is 19A.1B / 20.

[0012] The grey cloth has a weft density of 253 threads / 10cm, a warp tightness of 41.6, a weft tightness of 40.5, a weft-to-warp ratio of 0.97, and a plain weave structure.

[0013] Furthermore, in the dyeing and finishing process, singeing is direct burning with a flame intensity of 12.0 mbar, the temperature of the first continuous cooking is 85°C and the machine speed is 20 m / min, the temperature of the rope washing is 40°C, the machine speed is 300 m / min, the roller pressure is 1.5 bar, and the temperature of the second continuous cooking is 85°C and the machine speed is 30 m / min.

[0014] The drying temperature is 120°C and the speed is 20m / min.

[0015] The shearing knife distance for shearing is 0.45mm, the machine speed is 18m / min, the moistening amount is 40%, the machine speed is 20m / min, the calendering temperature is 110℃, the machine speed is 30m / min, the guide belt tension is 60%, the processing pressure of tank steaming is 1.0bar, and the processing time is 240 seconds.

[0016] Furthermore, the warping machine is a Benninger sectional warping machine.

[0017] Compared with the prior art, the beneficial technical effects of the present invention are:

[0018] The antistatic clothing fabric of the present invention has a comprehensive content of conductive filaments of 0.4%, and can pass not only the static charge test but also the point-to-point resistance test. It can meet the special industry needs of inflammable and explosive high-risk production, storage and transportation units such as oil fields, gas stations, flour mills and oil presses with high requirements for antistatic, has great application value, and can better meet safety needs. DETAILED DESCRIPTION

[0019] A method for producing a blended wool-silk interwoven antistatic clothing fabric. The blended wool-silk interwoven antistatic clothing fabric adopts raw materials and a comprehensive proportion of the raw materials: 50% 64S Australian wool, 39.6% 2D polyester fiber, 5% mulberry silk, 5% Tencel and 0.4% 20D nylon matrix conductive filament.

[0020] The specification parameters and organization structure of the blended wool and silk antistatic clothing fabric are as follows: the organization is 1 / 1 plain weave; the gram weight is 230g, the yarn count is 78 / 2*78 / 2 public count; the warp and weft density is 288*260 threads / 10cm.

[0021] The production method includes spinning process, weaving process and dyeing and finishing process. Specifically, the spinning process includes B412 blending, three needle combing before recombing, recombing, two needles after recombing, four needle combing before spinning, roving, spun yarn, one steaming yarn, winding, doubling, two-for-one twisting and two steaming yarns; the weaving process includes warping, drawing-in, weaving and grey cloth; the dyeing and finishing process includes singeing, one continuous boiling, rope scouring, opening width, two continuous boiling, drying, mid-inspection, trimming, shearing, moistening, calendering, tank steaming and finished products.

[0022] (1) In the spinning process, the warp yarn A and the weft yarn A are spun at 44 Nm / 1, twist direction Z, and twist degree 600 T / m; the yarn B is 20D nylon matrix conductive filament; the yarn A and the yarn B are spun together to form a 78 Nm / 2 yarn, twist direction S, and twist degree 1050 T / m.

[0023] (2) In the weaving process, the warping is done by a Benninger sectional warping machine, the tension of the single yarn is controlled at 18CN, cold sizing is added in the reeling process, the sizing amount is 40, and the reeling speed is less than 90m / min; the reeding, reeding and drop wire drawing are done by Swiss Stäubli equipment, and the three operations are completed at one time, with a speed of 260 yarns / min; the warp arrangement during weaving is 10A.1D.4B.[1C].11A.4B1C.2A.1D.8A.4B1C / 48, and the weft arrangement is 19A.1B / 20; the weft density of the grey fabric is 253 yarns / 10cm, the warp tightness is 41.6, the weft tightness is 40.5, the weft-to-warp ratio is 0.97, and the structure adopts plain weave.

[0024] Since the surface of plain weave is delicate, defects such as weft jumps and small flower jumps are prone to occur on the surface of the cloth. In order to control such defects on the surface of the cloth, it is necessary to reasonably set the relevant process parameters of the loom during the loom debugging process, and the process idea of ​​large opening and high tension is adopted in the loom debugging process.

[0025] (3) In the dyeing and finishing process, the singeing is direct burning and the flame intensity is 12.0 mbar; the temperature of the first continuous boiling is 85°C and the machine speed is 20 m / min; the temperature of the rope scouring is 40°C, the machine speed is 300 m / min, and the pressure of the pressure roller is 1.5 bar; the temperature of the second continuous boiling is 85°C, the machine speed is 30 m / min; the temperature of the drying is 120°C, and the machine speed is 20 m / min; the shearing blade distance of the shearing is 0.45 mm, and the machine speed is 18 m / min; the moisture supply is 40%, and the machine speed is 20 m / min; the temperature of the calendering is 110°C, the machine speed is 30 m / min, and the guide belt tension is 60%; the processing pressure of the tank steaming is 1.0 bar, and the processing time is 240 seconds.

[0026] In order to enable those skilled in the art to better understand the technical solution of the present invention, it will be further described in detail below in conjunction with specific embodiments.

[0027] Embodiment 1: A method for producing a blended wool-silk interwoven antistatic clothing fabric comprises the following steps: (1) Spinning process: The process flow comprises B412 blending, three needle combings before re-combing, re-combing, two needles after re-combing, four needle combings before spinning, coarse yarn, fine yarn, one-time steaming, winding, doubling, doubling, and two-time steaming.

[0028] The raw materials and proportions of the A yarn are 50% 64S Australian wool, 5% mulberry silk, 5% Tencel, and 39.6% 2D polyester fiber. The spun yarn produces 44Nm / 1 wool yarn with a twist of 600T / m and a twist direction of Z.

[0029] In the doubling process, 44Nm / 1 wool yarn (yarn A) and 20D nylon matrix conductive filament (yarn B) are twisted into 78Nm / 2, with a twist of 1050T / m and a twist direction of S.

[0030] (2) Weaving process: including warping, drawing-in, weaving and grey cloth.

[0031] The warping adopts Benninger sectional warping machine. To ensure the quality of the fabric, the warping tension is required to be kept small, and the single yarn tension is controlled at 18CN. Cold sizing needs to be added in the reversing process, and the sizing amount is 40, in order to increase the strength of the yarn and achieve the effect of taming the yarn hairiness. The reversing speed is controlled within 90m / min.

[0032] Drawing in the heald, reed and drop wires is done with Swiss Stäubli equipment, and the three operations are completed at one time, with a machine speed of 260 yarns / min.

[0033] During weaving, the warp yarns are arranged 10A.1D.4B.[1C].11A.4B1C.2A.1D.8A.4B1C / 48, and the weft yarns are arranged 19A.1B / 20, ensuring that the conductive yarns are arranged in a 0.8 cm grid shape.

[0034] Grey fabric has a weft density of 253 threads / 10cm, a warp tightness of 41.6, a weft tightness of 40.5, a weft-warp ratio of 0.97, and a plain weave. Plain weave is delicate, so defects such as weft jumps and small jumps are easy to appear on the surface. In order to control such defects on the surface, it is necessary to reasonably set the relevant process parameters of the loom during the loom debugging process. The specific process parameters are shown in Table 1. The loom debugging process adopts the process idea of ​​large opening and large tension.

[0035] Table 1 Fabric weaving process parameters

[0036] Process indicators Process parameters Rear beam height 6 Back beam depth 8 Warp stop height -2 Warp stop depth 3 Comprehensive time 325 Upper tension 40CN Comprehensive position 135-130mm Parking options SM

[0037] Note: The back beam height, back beam depth, warp stop frame height and warp stop frame depth are the actual production time.

[0038] (3) Dyeing and finishing process: including singeing, primary continuous boiling, rope scouring, opening, secondary continuous boiling, drying, intermediate inspection, trimming, shearing, moistening, calendering, tank steaming, and finished product.

[0039] The singeing adopts direct burning with a flame intensity of 12.0mbar; the temperature of the first continuous boiling is 85℃ and the machine speed is 20m / min; the temperature of the rope washing is 40℃, the machine speed is 300m / min, and the pressure of the pressure roller is 1.5bar; the temperature of the second continuous boiling is 85℃, the machine speed is 30m / min; the temperature of the drying is 120℃, and the machine speed is 20m / min; the shearing knife distance of shearing is 0.45mm, and the machine speed is 18m / min; the moistening amount is 40%, and the machine speed is 20m / min; the calendering temperature is 110℃, the machine speed is 30m / min, and the guide belt tension is 60%; the processing pressure of tank steaming is 1.0bar, and the processing time is 240 seconds.

[0040] The blended wool and silk interwoven antistatic clothing fabric obtained in Example 1 was subjected to a point-to-point resistance test according to GB12014-2019 "Protective Clothing Antistatic Clothing", and an electrostatic charge test was performed according to GB / T12703.2-2021 "Evaluation of Electrostatic Properties of Textiles Part 1: Electrostatic Voltage Half-Life".

[0041] The point-to-point resistance test result is: 1.66×10 10 Ω, in the standard range 1×10 5 ~1×10 31 Ω, it is considered qualified. The static charge test results are: friction charge surface density (Uc / m 2 ): The initial value is 0.7, which meets the standard of ≤3.0; the value after washing 10 times is 2.2, which meets the standard of ≤3.0, and is judged to be qualified.

[0042] The antistatic clothing fabric of the present invention can not only pass the static charge test, but also pass the point-to-point resistance test, and can meet the special industry needs of inflammable and explosive high-risk production, storage and transportation units such as oil fields, gas stations, flour mills and oil presses with high requirements for antistatic, has great application value, and can better meet safety needs.

[0043] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. When the conductive fiber content (increases from 0.4% to 1%) increases, the antistatic performance will be greatly improved. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A blended wool and silk antistatic clothing fabric, It is characterized in that The raw materials and their comprehensive proportions used are: 50% 64S Australian wool, 39.6% 2D polyester fiber, 5% mulberry silk, 5% Tencel, and 0.4% 20D nylon matrix conductive filament; The organization is 1 / 1 plain weave; The weight is 230g, the yarn count is 78 / 2*78 / 2; The warp and weft density is 288*260 threads / 10cm.

2. A method for making the blended wool and silk antistatic clothing fabric according to claim 1, It is characterized in that The invention comprises spinning process, weaving process and dyeing and finishing process. The spinning process comprises B412 blending, three needle combings before re-combing, re-combing, two needle combings after re-combing, four needle combings before spinning, coarse yarn, spun yarn, one-time steaming, bobbin winding, paralleling, double twisting and two-time steaming. The weaving process comprises warping, drawing-in, weaving and grey cloth. The dyeing and finishing process comprises singeing, one-time continuous boiling, rope-shaped washing, opening width, two-time continuous boiling, drying, center inspection, trimming, shearing, moistening, calendering, tank steaming and finished product.

3. The method for making the blended wool-silk interwoven antistatic clothing fabric according to claim 2, It is characterized in that In the spinning process, warp D yarn and weft B yarn are spun at 44Nm / 1, twist direction Z, and twist degree 600T / m; B yarn is 20D nylon matrix conductive filament; A yarn and B yarn are spun together to form 78Nm / 2 yarn, twist direction S, and twist degree 1050T / m.

4. The method for making the blended wool-silk interwoven antistatic clothing fabric according to claim 3, It is characterized in that In the weaving process, warping is done by a warping machine, the tension of the single yarn is controlled at 18CN, cold sizing is added in the reversing process, the sizing amount is 40, and the reversing speed is <90m / min; Drawing in the heald, reed and drop wires is done with Swiss Stäubli equipment, and the three operations are completed at one time, with a machine speed of 260 yarns / min. When weaving, the warp yarn arrangement is 10A.1D.4B.[1C].11A.4B1C.2A.1D.8A.4B1C / 48, and the weft yarn arrangement is 19A.1B / 20; The grey cloth has a weft density of 253 threads / 10cm, a warp tightness of 41.6, a weft tightness of 40.5, a weft-to-warp ratio of 0.97, and a plain weave structure.

5. The method for making the blended wool-silk interwoven antistatic clothing fabric according to claim 4, It is characterized in that In the dyeing and finishing process, the singeing is direct burning with a flame intensity of 12.0mbar, the temperature of the first continuous cooking is 85℃, the speed is 20m / min, the temperature of the rope washing is 40℃, the speed is 300m / min, the pressure of the roller is 1.5bar, and the temperature of the second continuous cooking is 85℃, the speed is 30m / min; The drying temperature is 120°C and the speed is 20m / min; The shearing knife distance for shearing is 0.45mm, the machine speed is 18m / min, the moistening amount is 40%, the machine speed is 20m / min, the calendering temperature is 110℃, the machine speed is 30m / min, the guide belt tension is 60%, the processing pressure of tank steaming is 1.0bar, and the processing time is 240 seconds.

6. The method for making the blended wool-silk interwoven antistatic clothing fabric according to claim 5, It is characterized in that The warping machine is a Benninger sectional warping machine.

Citation Information

Patent Citations

  • Permanent antistatic worsted fabric and production method thereof

    CN101643963A

  • Coal mine protective clothing fabric and preparation method thereof

    CN103061000A

  • Bacteriostatic anti-ultraviolet anti-static protective tooling fabric and preparation method thereof

    CN114232180A

  • method blending producing antistatic spinning wool fabric by conductive chinlon and wool, polyester fibre

    CN1724733A

  • Anti-static wool or fibric of wool product and its processing method

    CN1912216A