Preparation method of antibacterial modified polyester fiber blended woven fabric

Through the blending and melt spinning processing of antibacterial modified polyester fiber and fine wool cotton fiber, combined with the woven process, the existing antibacterial textile fabric process is solved, and the efficient antibacterial performance and top-breaking of the fabric is achieved Improve performance and maintain excellent results after multiple washes.

CN118979331AActive Publication Date: 2024-11-19FUZHOU SHENGHAO TEXTILE TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410947525.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-19
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing antibacterial textile fabrics are complex and costly, difficult to popularize, and their antibacterial properties are reduced after multiple washes.

Method used

Antibacterial modified polyester fiber and lint cotton fiber are blended, and the mixture of itaconic acid, 1,2-propylene glycol, hydroquinone and p-toluenesulfonic acid, azobisisobutyronitrile, 4-vinylbenzyl chloride , reaction of pentamethyldivinyltriamine and octadecane to form benzyl chloride grafted polyester, and melt-spinning process is carried out under a nitrogen atmosphere, fabric is prepared in combination with a woven process, and cross-linking network and hydrophobic long chain to improve antibacterial performance.

Benefits of technology

It improves the top-breaking performance and antibacterial properties of the fabric, and maintains excellent antibacterial properties after multiple washes, reducing process complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946120160000091
    Figure BDA0004946120160000091
Patent Text Reader

Abstract

The invention relates to the technical field of antibacterial fabrics, in particular to a preparation method of an antibacterial modified polyester fiber blended woven fabric. According to the fabric obtained through the preparation method of the antibacterial modified polyester fiber blended woven fabric, antibacterial modified polyester fibers and fine staple cotton fibers are blended to obtain blended yarns, then the blended yarns are subjected to a weaving process, and the antibacterial modified polyester fibers are obtained by melt spinning processing of a mixture of antibacterial modified polyester and polyester chips. The antibacterial modified polyester fiber blended woven fabric has excellent bursting performance, the grade of the antibacterial modified polyester fiber blended woven fabric can still reach 4.5 after the antibacterial modified polyester fiber blended woven fabric is rubbed for 500 times, the antibacterial modified polyester fiber blended woven fabric has excellent antibacterial performance, and most importantly, the antibacterial performance of the antibacterial modified polyester fiber blended woven fabric can still be maintained at a relatively excellent level after the antibacterial modified polyester fiber blended woven fabric is washed with water for multiple times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibacterial fabrics, and in particular to a method for preparing an antibacterial modified polyester fiber blended woven fabric. Background Art

[0002] Nowadays, living standards have greatly improved. People's requirements for clothing are not only to cover the body so simply, but also to greatly increase the demand for some special properties of clothing, such as comfortable functions. The most common and popular properties now are UV protection, moisture absorption and quick drying, antibacterial, and winter clothing needs to be windproof and warm.

[0003] Patent technology document CN201910794660.4 discloses a waterproof and UV-proof textile fabric, which comprises an outer layer, a middle layer and an inner layer, wherein the outer layer is treated with silicone plasma and UV-proof, and the middle layer is treated with pores and oxygen plasma; the middle layer is a blend of acrylic and linen fibers. The waterproof and UV-proof textile fabric prepared by the invention adopts a special process and fabric, so that the fabric has the functions of moisture-proof, sun-proof and waterproof and breathable.

[0004] With the continuous improvement of modern hygiene standards and people's increasing attention to health, antibacterial clothing has gradually come into the public eye. Patent technology document CN202011602592.6 discloses a method for preparing antibacterial knitted fabrics, which is made by adding spandex to the blended yarns blended from antibacterial polyester fiber and modal fiber to obtain a knitted single-sided cloth, and then undergoing pre-setting, pre-treatment, dyeing, dehydration, slitting, drying, setting and pre-shrinking to obtain the antibacterial knitted fabric; the antibacterial knitted fabric includes the following components: antibacterial polyester fiber, modal fiber, spandex; the present invention utilizes coordination technology to firmly control Ag+ in the polyester fiber, thereby enhancing the antibacterial and deodorizing efficiency of the antibacterial agent and its permanence in the polyester fiber, improving the sustainability of the antibacterial property, and having excellent performance, health and environmental protection. However, its process key positions are complex and the cost is high, which is not conducive to popularization. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a method for preparing an antibacterial modified polyester fiber blended woven fabric, so as to provide a fabric with good antibacterial properties.

[0006] Based on the above purpose, the present invention provides a method for preparing an antibacterial modified polyester fiber blended woven fabric, wherein the antibacterial modified polyester fiber blended woven fabric is prepared by blending antibacterial modified polyester fiber and fine cotton fiber to obtain blended yarn and then undergoing a weaving process; the antibacterial modified polyester fiber is obtained by melt spinning a mixture of antibacterial modified polyester and polyester chips;

[0007] The preparation steps of the antibacterial modified polyester are as follows:

[0008] S1: Mix itaconic acid, 1,2-propylene glycol, hydroquinone and p-toluenesulfonic acid, heat to 160-170°C, reflux for 12-14h, extract, filter and rotary evaporate to obtain unsaturated polyester;

[0009] S2: adding unsaturated polyester to N,N-dimethylacetamide, adding azobisisobutyronitrile under nitrogen atmosphere, heating to 70-80°C, adding 4-vinylbenzyl chloride, stirring to react for 16-20h, washing, and drying to obtain benzyl chloride grafted polyester;

[0010] S3: Add the benzyl chloride grafted polyester to N-methylpyrrolidone, stir for 10-20 minutes, then add pentamethyldiethylenetriamine, stir and react at room temperature for 1-2 hours, then add iodooctadecane, continue stirring for 6-8 hours, and rotary evaporate to obtain the antibacterial modified polyester.

[0011] Preferably, the length of the fine cotton fiber is 35-40 mm and the fineness is 1.5-1.7 dtex.

[0012] Preferably, the blending ratio of the antibacterial modified polyester fiber and the fine cotton fiber is 20-35:65-80.

[0013] Preferably, in step S1, the weight ratio of itaconic acid, 1,2-propylene glycol, hydroquinone and p-toluenesulfonic acid is 120-140:80-90:1-1.1:1-1.1.

[0014] Preferably, in step S2, the weight ratio of the unsaturated polyester, N,N-dimethylacetamide, azobisisobutyronitrile and 4-vinylbenzyl chloride is 3-4:50-60:0.1-0.3:5-10.

[0015] Preferably, in step S3, the weight ratio of the benzyl chloride grafted polyester, N-methylpyrrolidone, pentamethyldiethylenetriamine and iodooctadecane is 1-5:30-40:0.3-0.8:0.5-1.

[0016] Preferably, the polyester chips are PET polyester chips.

[0017] Preferably, the specific preparation method of the antibacterial modified polyester fiber is: blending the antibacterial modified polyester and polyester chips, then spinning the mixture at 260-270°C, at a spinning speed of 3000m / min, and then stretching at a ratio of 1.5-2 to obtain the antibacterial modified polyester fiber.

[0018] Preferably, the weight ratio of the antibacterial modified polyester to the polyester chips is 1-3:10.

[0019] Preferably, the density of the antibacterial modified polyester fiber blended woven fabric obtained by weaving is 140-150g / m 2 .

[0020] Preferably, the antibacterial modified polyester fiber blended woven fabric obtained by weaving is a plain knitted fabric.

[0021] Beneficial effects of the present invention:

[0022] (1) The present invention uses pentamethyldiethylenetriamine to modify polyester, thereby improving the density of the cross-linked network, thereby improving the bursting performance of the fabric, and introducing a large number of active sites into the cross-linked network. Through subsequent quaternization treatment, a large number of cationic groups are introduced, thereby improving the antibacterial performance of the fabric.

[0023] (2) The present invention introduces long hydrophobic chains by modifying polyester with iodooctadecane, and the long hydrophobic chains are distributed in the cross-linked network, further improving the antibacterial and bursting properties of the fabric; most importantly, the antibacterial properties of the fabric remain at a relatively excellent level after multiple washings.

[0024] (3) The present invention modifies polyester by using iodooctadecane and pentamethyldiethylenetriamine, thereby introducing cationic groups and long hydrophobic chains. The two groups together promote the improvement of the antibacterial and bursting properties of the fabric, and the fabric finally obtained still maintains relatively excellent antibacterial properties after multiple washings. DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0026] The properties of the raw materials used in the embodiments of the present invention and the comparative examples are as follows: the length of the fine-staple cotton fiber is 38 mm and the fineness is 1.6 dtex;

[0027] Example 1: A method for preparing an antibacterial modified polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0028] (1) 120 g of itaconic acid, 80 g of 1,2-propylene glycol, 1 g of hydroquinone and 1 g of p-toluenesulfonic acid were mixed, the temperature was raised to 160° C., refluxed for 12 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0029] (2) 3 g of unsaturated polyester was added to 50 g of N,N-dimethylacetamide, and 0.1 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 70° C., and 5 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 16-20 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0030] (3) 1 g of benzyl chloride grafted polyester was added to 30 g of N-methylpyrrolidone, stirred for 10 min, then 0.3 g of pentamethyldiethylenetriamine was added, stirred and reacted at room temperature for 1 h, then 0.5 g of iodooctadecane was added, stirring was continued for 6 h, and rotary evaporation was performed to obtain an antibacterial modified polyester;

[0031] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 1:10, spinning the mixture at 260° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 1.5 to obtain an antibacterial modified polyester fiber;

[0032] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 20:80, and then woven using a WF-52CJD computer flat knitting machine, scouring, washing, and shaping to obtain a density of 140 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0033] Example 2: A method for preparing an antibacterial modified polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0034] (1) 130 g of itaconic acid, 85 g of 1,2-propylene glycol, 1.05 g of hydroquinone and 1.05 g of p-toluenesulfonic acid were mixed, heated to 165° C., refluxed for 13 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0035] (2) 3.5 g of unsaturated polyester was added to 55 g of N,N-dimethylacetamide, and 0.2 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 75° C., and 7.5 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 18 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0036] (3) 3 g of benzyl chloride grafted polyester was added to 35 g of N-methylpyrrolidone, stirred for 15 min, then 0.5 g of pentamethyldiethylenetriamine was added, stirred and reacted at room temperature for 2 h, then 0.75 g of iodooctadecane was added, stirring was continued for 7 h, and rotary evaporation was performed to obtain an antibacterial modified polyester;

[0037] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 2:10, spinning the mixture at 265° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 2 to obtain an antibacterial modified polyester fiber;

[0038] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 30:70, and then woven using a WF-52CJD computerized flat knitting machine, scouring, washing, and shaping to obtain a density of 150 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0039] Example 3: A method for preparing an antibacterial modified polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0040] (1) 135 g of itaconic acid, 88 g of 1,2-propylene glycol, 1.1 g of hydroquinone and 1.1 g of p-toluenesulfonic acid were mixed, heated to 170° C., refluxed for 14 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0041] (2) 4 g of unsaturated polyester was added to 55 g of N,N-dimethylacetamide, and 0.2 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 75° C., and 8 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 19 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0042] (3) 4 g of benzyl chloride grafted polyester was added to 40 g of N-methylpyrrolidone, stirred for 18 min, then 0.6 g of pentamethyldiethylenetriamine was added, stirred and reacted at room temperature for 2 h, then 1 g of iodooctadecane was added, stirring was continued for 8 h, and rotary evaporation was performed to obtain an antibacterial modified polyester;

[0043] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 3:10, spinning the mixture at 270° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 2 to obtain an antibacterial modified polyester fiber;

[0044] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 25:75, and then woven using a WF-52CJD computerized flat knitting machine, scouring, washing, and shaping to obtain a density of 143 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0045] Example 4: A method for preparing an antibacterial modified polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0046] (1) 140 g of itaconic acid, 90 g of 1,2-propylene glycol, 1.1 g of hydroquinone and 1.1 g of p-toluenesulfonic acid were mixed, heated to 170° C., refluxed for 14 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0047] (2) 4 g of unsaturated polyester was added to 60 g of N,N-dimethylacetamide, and 0.3 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 80° C., and 10 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 20 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0048] (3) 5 g of benzyl chloride grafted polyester was added to 40 g of N-methylpyrrolidone, stirred for 20 min, then 0.8 g of pentamethyldiethylenetriamine was added, stirred and reacted at room temperature for 2 h, then 1 g of iodooctadecane was added, stirring was continued for 8 h, and rotary evaporation was performed to obtain an antibacterial modified polyester;

[0049] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 3:10, spinning the mixture at 270° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 2 to obtain an antibacterial modified polyester fiber;

[0050] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 35:65, and then woven using a WF-52CJD computer flat knitting machine, scouring, washing, and shaping to obtain a density of 147 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0051] Comparative Example 1: A method for preparing an antibacterial polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0052] (1) 130 g of itaconic acid, 85 g of 1,2-propylene glycol, 1.05 g of hydroquinone and 1.05 g of p-toluenesulfonic acid were mixed, heated to 165° C., refluxed for 13 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0053] (2) 3.5 g of unsaturated polyester was added to 55 g of N,N-dimethylacetamide, and 0.2 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 75° C., and 7.5 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 18 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0054] (3) 3 g of benzyl chloride grafted polyester was added to 35 g of N-methylpyrrolidone, stirred for 15 min, then 0.37 g of tetramethylpropylenediamine was added, stirred and reacted at room temperature for 2 h, then 0.75 g of iodooctadecane was added, stirring was continued for 7 h, and rotary evaporation was performed to obtain an antibacterial modified polyester;

[0055] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 2:10, spinning the mixture at 265° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 2 to obtain an antibacterial modified polyester fiber;

[0056] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 30:70, and then woven using a WF-52CJD computerized flat knitting machine, scouring, washing, and shaping to obtain a density of 150 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0057] Comparative Example 2: A method for preparing an antibacterial polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0058] (1) 130 g of itaconic acid, 85 g of 1,2-propylene glycol, 1.05 g of hydroquinone and 1.05 g of p-toluenesulfonic acid were mixed, heated to 165° C., refluxed for 13 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0059] (2) 3.5 g of unsaturated polyester was added to 55 g of N,N-dimethylacetamide, and 0.2 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 75° C., and 7.5 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 18 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0060] (3) 3 g of benzyl chloride grafted polyester was added to 35 g of N-methylpyrrolidone, stirred for 15 min, then 0.5 g of pentamethyldiethylenetriamine was added, stirred and reacted at room temperature for 2 h, then 0.31 g of ethyl iodide was added, stirring was continued for 7 h, and rotary evaporation was performed to obtain an antibacterial modified polyester;

[0061] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 2:10, spinning the mixture at 265° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 2 to obtain an antibacterial modified polyester fiber;

[0062] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 30:70, and then woven using a WF-52CJD computerized flat knitting machine, scouring, washing, and shaping to obtain a density of 150 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0063] Comparative Example 3: A method for preparing an antibacterial polyester fiber blended woven fabric, the specific preparation steps are as follows:

[0064] (1) 130 g of itaconic acid, 85 g of 1,2-propylene glycol, 1.05 g of hydroquinone and 1.05 g of p-toluenesulfonic acid were mixed, heated to 165° C., refluxed for 13 h, extracted, filtered, and rotary evaporated to obtain an unsaturated polyester;

[0065] (2) 3.5 g of unsaturated polyester was added to 55 g of N,N-dimethylacetamide, and 0.2 g of azobisisobutyronitrile was added under a nitrogen atmosphere. The temperature was raised to 75° C., and 7.5 g of 4-vinylbenzyl chloride was added. The mixture was stirred for reaction for 18 h, washed, and vacuum dried at 80° C. for 24 h to obtain a benzyl chloride grafted polyester;

[0066] (3) 3 g of benzyl chloride grafted polyester was added to 35 g of N-methylpyrrolidone, stirred for 15 min, then 0.17 g of trimethylamine was added, stirred and reacted at room temperature for 2 h, and rotary evaporated to obtain antibacterial modified polyester;

[0067] (4) blending the antibacterial modified polyester and PET polyester chips at a weight ratio of 2:10, spinning the mixture at 265° C. at a spinning speed of 3000 m / min, and then stretching at a ratio of 2 to obtain an antibacterial modified polyester fiber;

[0068] (5) The antibacterial modified polyester fiber and the fine cotton fiber were blended at a blending ratio of 30:70, and then woven using a WF-52CJD computerized flat knitting machine, scouring, washing, and shaping to obtain a density of 150 g / m 2 Antibacterial modified polyester fiber blended woven fabric.

[0069] Performance Testing

[0070] Bursting performance: According to GB / T 19976-2005 “Determination of bursting strength of textiles - Steel ball method”, a YG031DC marble bursting strength tester (manufactured by Quanzhou Meibang Instrument Co., Ltd.) was used to test the bursting performance of the samples obtained in the embodiments and comparative examples. The test results are shown in Table 1.

[0071] Anti-pilling performance: According to GB / T 4802.2-2008 “Determination of pilling properties of textile fabrics Part 2: Modified Martindale method”, the pilling performance of the samples obtained in the embodiments and comparative examples was tested using a YG502 fabric pilling tester (produced by Quanzhou Meibang Instrument Co., Ltd.). The test results are shown in Table 1.

[0072] Antibacterial property: The samples obtained in the embodiments and comparative examples were cut into pieces, and 0.1 g of each sample was taken. According to GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the antibacterial properties of the samples obtained in the embodiments and comparative examples were tested with Gram-positive bacteria Staphylococcus aureus and Gram-negative bacteria Escherichia coli as test strains. The test results are shown in Table 1; then the samples obtained in the embodiments and comparative examples were washed with water for 30 times, and after drying, each sample was cut into pieces and 0.1 g was taken, and the antibacterial properties were tested here. The test results are shown in Table 1.

[0073] Table 1 Performance test results

[0074]

[0075] It can be seen from Examples 1-4 in Table 1 that the fabric obtained by the preparation method of an antibacterial modified polyester fiber blended woven fabric of the present invention has good bursting performance, and the rating after 500 frictions can still reach 4.5; and has excellent antibacterial performance, and most importantly, after multiple washings, it can still maintain relatively excellent antibacterial performance.

[0076] It can be seen from Example 2 and Comparative Example 1 in Table 1 that the present invention improves the density of the cross-linked network by modifying the polyester with pentamethyldiethylenetriamine, thereby improving the bursting performance of the fabric, and introduces a large number of active sites into the cross-linked network. Through subsequent quaternization treatment, a large number of cationic groups are introduced, thereby improving the antibacterial performance of the fabric.

[0077] It can be seen from Example 2 and Comparative Example 2 in Table 1 that the present invention introduces hydrophobic long chains by modifying polyester with iodooctadecane, and the hydrophobic long chains are distributed in the cross-linked network, which further improves the antibacterial and bursting properties of the fabric; most importantly, the antibacterial properties of the fabric remain at a relatively excellent level after multiple washings.

[0078] It can be seen from Example 2 and Comparative Example 3 in Table 1 that the present invention modifies polyester by using iodooctadecane and pentamethyldiethylenetriamine, and introduces cationic groups while also introducing hydrophobic long chains. The two together promote the improvement of the antibacterial and bursting properties of the fabric, and the fabric finally obtained still maintains relatively excellent antibacterial properties after multiple washings.

[0079] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing an antibacterial modified polyester fiber blended woven fabric, characterized in that: The antibacterial modified polyester fiber blended woven fabric is obtained by blending antibacterial modified polyester fiber and fine cotton fiber to obtain blended yarn and then undergoing a weaving process; the antibacterial modified polyester fiber is obtained by melt spinning a mixture of antibacterial modified polyester and polyester chips; The preparation steps of the antibacterial modified polyester are as follows: S1: Mix itaconic acid, 1,2-propylene glycol, hydroquinone and p-toluenesulfonic acid, heat to 160-170°C, reflux for 12-14h, extract, filter and rotary evaporate to obtain unsaturated polyester; S2: adding unsaturated polyester to N,N-dimethylacetamide, adding azobisisobutyronitrile under nitrogen atmosphere, heating to 70-80°C, adding 4-vinylbenzyl chloride, stirring and reacting for 16-20h, washing, and drying to obtain benzyl chloride grafted polyester; S3: Add the benzyl chloride grafted polyester to N-methylpyrrolidone, stir for 10-20 minutes, then add pentamethyldiethylenetriamine, stir and react at room temperature for 1-2 hours, then add iodooctadecane, continue stirring for 6-8 hours, and rotary evaporate to obtain the antibacterial modified polyester.

2. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The length of the fine cotton fiber is 35-40 mm, and the fineness is 1.5-1.7 dtex.

3. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The blending ratio of the antibacterial modified polyester fiber and the fine cotton fiber is 20-35:65-80.

4. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The weight ratio of itaconic acid, 1,2-propylene glycol, hydroquinone and p-toluenesulfonic acid in step S1 is 120-140:80-90:1-1.1:1-1.

1.

5. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The weight ratio of the unsaturated polyester, N,N-dimethylacetamide, azobisisobutyronitrile and 4-vinylbenzyl chloride in step S2 is 3-4:560:0.1-0.3:5-10.

6. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The weight ratio of the benzyl chloride grafted polyester, N-methylpyrrolidone, pentamethyldiethylenetriamine and iodooctadecane in step S3 is 1-5:30-40:0.3-0.8:0.5-1.

7. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The polyester chips are PET polyester chips.

8. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The specific preparation method of the antibacterial modified polyester fiber is: blending the antibacterial modified polyester and polyester chips, spinning the mixture at 260-270°C, with a spinning speed of 3000m / min, and then stretching at a ratio of 1.5-2 times to obtain the antibacterial modified polyester fiber.

9. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The weight ratio of the antibacterial modified polyester to the polyester chips is 1-3:

10.

10. The method for preparing the antibacterial modified polyester fiber blended woven fabric according to claim 1, characterized in that: The density of the antibacterial modified polyester fiber blended woven fabric obtained by weaving is 140-150g / m 2 .

Citation Information

Patent Citations

  • Preparation method of long-chain alkane quaternization antibacterial agent, and product and application of antibacterial agent

    CN109503834A

  • Preparation method of antistatic and antibacterial fabric

    CN110616472A

  • Anti-mite antibacterial knitted gigging fabric and preparation method thereof

    CN116084079A

  • High-temperature-resistant polyurethane anti-condensation airtight plugging material and preparation method thereof

    CN117126370A

  • Quick-dry fabric special for clothes and processing technology of quick-dry fabric

    CN117418350A