Dyeing method for dyeing white velvet into olive green by adopting lanasol dye

By combining Lanas dye and specific auxiliaries with temperature and temperature control, the problems of damage and color difference in the dyeing process of white velvet were solved, achieving uniform coloring and high color fixation.

CN118979395APending Publication Date: 2024-11-19TONGXIANG OUHE TEXTILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411281856.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing white velvet dyeing processes cause significant damage to fibers, resulting in poor hand feel, low dyeing rate, and insufficient color uniformity and color fastness. In particular, dark colors are prone to color difference and fading after dyeing.

Method used

The dyeing process involves using Lannes dye in combination with a specific ratio of FFA defoaming and penetrating agent, Abbey B leveling agent, soda ash, formic acid, and cashmere softener. The dyeing is carried out by controlling the temperature and the rate of heating and cooling. An olive green color is formed using CN dye, Lannes Golden Yellow CE, Lannes Red CE, and Lannes Blue CE. The washing temperature and number of washes are controlled.

Benefits of technology

It reduces damage to the white down, improves the feel and color uniformity, avoids color difference, enhances color fastness, and ensures dyeing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979395A_ABST
    Figure CN118979395A_ABST
Patent Text Reader

Abstract

The invention discloses a dyeing method for dyeing white velvet into olive green by adopting lanasol dye, which comprises the following steps: S1, adding the white velvet and dye liquor into a dye vat according to the dye liquor bath ratio of 1: 15; s2, the temperature is increased to 40 DEG C, 0.45-0.55% of an FFA defoaming penetrant and 1.45-1.55% of an Albegal B leveling agent are added on the basis of the mass of the white velvet, olive green lanasol dye is added after 5 minutes, and the temperature is maintained for 10 minutes; s3, raising the temperature to 70 DEG C at the speed of 1 DEG C / 1.5 min, raising the temperature to 95 DEG C at the speed of 1 DEG C / 1 min after 20 min, and maintaining the temperature for 40 min; s4, the temperature is reduced to 80 DEG C, 1.45-1.55% of sodium carbonate is added on the basis of the mass of the white velvet, washing is carried out after the white velvet is kept for 20 min, and the temperature is reduced to 40 DEG C; and S5, adding 0.45-0.55% of formic acid and 0.45-0.55% of a cashmere softening and slipping agent on the basis of the mass of the white cashmere, and directly discharging the white cashmere from the machine after 20 minutes to finish dyeing. The coloring uniformity is good, the consistency of the overall color sense can be improved, the color fastness is good, and the color fading phenomenon is not prone to occurring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of textile printing and dyeing, and in particular to a dyeing method for dyeing white velvet into olive green by using lanner dye. Background Art

[0002] White cashmere is a kind of cashmere with the characteristics of green and grayish white, without the inclusion of variegated hair. The fiber of white cashmere is slender, strong in tensile strength, good in gloss, and softer than other cashmere. It also has a high cashmere yield and a rock sugar color, which makes it suitable for dyeing of all colors. At present, when dyeing white cashmere, it is directly dyed with a dye. This dyeing process causes great damage to the white cashmere fiber, resulting in a poor hand feel of the white cashmere. At the same time, the dyeing rate of this process is low, and the color uniformity is poor, resulting in inconsistent overall color of the dyed white cashmere. Especially after dyeing dark colors such as olive green, the color difference is serious, and the color fastness is poor, and it is easy to fade. Summary of the invention

[0003] In order to solve one or some technical problems existing in the prior art, the purpose of the present application is to provide a dyeing method for dyeing white wool into olive green using lanner dye, which can reduce the damage of white wool, improve the feel of white wool, and have good coloring uniformity, which can improve the consistency of overall color, avoid color difference, have good color fastness, and is not easy to fade.

[0004] In order to solve the above existing technical problems, the purpose of the present application is achieved by adopting the following technical solution: a dyeing method for dyeing white velvet into olive green using lanner dye, comprising the following steps:

[0005] S1: Add white wool and dye solution into the dyeing vat, with the dye solution bath ratio being 1:15;

[0006] S2: Raise the temperature to 40°C, add 0.45-0.55% FFA degassing penetrant and 1.45-1.55% Abaige B leveling agent based on the mass of white wool, add olive green lanner dye after 5 minutes, and maintain for 10 minutes;

[0007] S3: Raise the temperature to 70°C at a rate of 1°C / 1.5 min, then raise the temperature to 95°C at a rate of 1°C / 1 min after 20 minutes, and maintain for 40 minutes;

[0008] S4: Cool down to 80°C, add 1.45-1.55% soda ash based on the mass of white wool, keep it for 20 minutes, then wash it with water and lower the temperature to 40°C;

[0009] S5: Based on the quality of white cashmere, add 0.45-0.55% formic acid and 0.45-0.55% cashmere softener, and then exit the machine directly after 20 minutes to complete dyeing.

[0010] Among them, the control of temperature, the control of heating and cooling rates, and the control of temperature maintenance time play a very important role, ensuring the smooth progress of the entire dyeing process and improving the dyeing quality.

[0011] Preferably, in step S2, based on the mass of white velvet, the olive green lanner dye is 1% CN dye, 1.19% lanner golden CE, 0.45% lanner red CE and 0.83% lanner blue CE, forming a pure olive green color with good coloring uniformity, which can improve the consistency of the overall color sense and avoid color difference.

[0012] Preferably, the CN dye contains 25-30% ethoxylated iso-rich C9-11 alcohol, 20-25% ethoxylated tridecanol, 3-10% oligomeric D-pyranose C10-16-alkyl glycoside, and the rest is water. The color fastness is good and fading is not easy to occur.

[0013] Preferably, in step S4, the wool is first washed twice with water at 60°C and then washed twice with water at room temperature. The overall temperature is lowered during washing to eliminate excess dye attached to the surface and ensure the coloring effect of the white wool.

[0014] Preferably, the cashmere softening agent in step S5 contains 4% ethoxylated isotriacontanol, 1% diethylene glycol butyl ether, 10% silicone oil, 0.2% acetic acid, and the rest is water, which can reduce the damage to the white cashmere and improve the feel of the white cashmere.

[0015] Preferably, 0.45% FFA degassing penetrant and 1.45% Abaige B leveling agent are added in step S2; 1.45% soda ash is added in step S4; and 0.45% formic acid and 0.45% cashmere softening agent are added in step S5.

[0016] Preferably, 0.5% FFA degassing penetrant and 1.5% Abaige B leveling agent are added in step S2; 1.5% soda ash is added in step S4; and 0.5% formic acid and 0.5% cashmere softening agent are added in step S5.

[0017] Preferably, 0.55% FFA degassing penetrant and 1.55% Abaige B leveling agent are added in step S2; 1.55% soda ash is added in step S4; and 0.55% formic acid and 0.55% cashmere softening agent are added in step S5.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] A dyeing method for dyeing white wool into olive green by using lanner dye adopts the above technical scheme. The cashmere softener in the scheme can reduce the damage of white wool and improve the feel of white wool; CN dye and lanner dye are combined to form a pure olive green color, so that the coloring uniformity is good, the consistency of the overall color sense can be improved, and color difference can be avoided; the CN dye in the scheme has good color fastness and is not prone to fading; the control of temperature, the control of heating and cooling rate and the control of temperature maintenance time play a very important role in the scheme, ensuring the smooth progress of the entire dyeing process and improving the dyeing quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0021] Below, the present application is further described in conjunction with the accompanying drawings and specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0022] In the description of the present application, it should be understood that the terms "up", "down", "left", "right", etc., indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present application.

[0023] Embodiment 1:

[0024] like Figure 1 As shown, a dyeing method for dyeing white velvet into olive green using lanner dye comprises the following steps:

[0025] S1: Add white wool and dye solution into the dyeing vat, with the dye solution bath ratio being 1:15;

[0026] S2: Raise the temperature to 40°C, add 0.45% FFA degassing penetrant and 1.45% Abaige B leveling agent based on the mass of white wool, add olive green lanner dye after 5 minutes, and maintain for 10 minutes;

[0027] S3: Raise the temperature to 70°C at a rate of 1°C / 1.5 min, then raise the temperature to 95°C at a rate of 1°C / 1 min after 20 minutes, and maintain for 40 minutes;

[0028] S4: Cool down to 80°C, add 1.45% soda ash based on the mass of white wool, keep for 20 minutes, then wash with water and lower the temperature to 40°C;

[0029] S5: Based on the quality of white cashmere, add 0.45% formic acid and 0.45% cashmere softener, and then exit the machine directly after 20 minutes to complete dyeing.

[0030] In this embodiment, the added components of FFA degassing penetrant, Abaige B leveling agent, soda ash, formic acid and cashmere softening agent are relatively low.

[0031] In step S2, the olive green lanner dye is based on the mass of white velvet, and is 1% CN dye, 1.19% lanner golden CE, 0.45% lanner red CE and 0.83% lanner blue CE. A pure olive green color is formed, and the coloring uniformity is good, which can improve the consistency of the overall color sense and avoid color difference. The CN dye contains 25-30% ethoxylated iso-rich C9-11 alcohol, 20-25% ethoxylated tridecanol, 3-10% oligomeric D-pyranose C10-16-alkyl glycoside, and the rest is water. The color fastness is good and fading is not easy to occur.

[0032] In step S4, the 60°C water is used for washing twice, and then the room temperature water is used for washing twice. The overall temperature is lowered during washing, and the excess dye attached to the surface is eliminated to ensure the coloring effect of the white wool.

[0033] The cashmere softening agent in step S5 contains 4% ethoxylated isotriacontanol, 1% diethylene glycol butyl ether, 10% silicone oil, 0.2% acetic acid, and the rest is water, which can reduce the damage to the white cashmere and improve the feel of the white cashmere.

[0034] The control of temperature, the control of heating and cooling rates, and the control of temperature maintenance time play a very important role in this scheme, ensuring the smooth progress of the entire dyeing process and improving the dyeing quality.

[0035] Embodiment 2:

[0036] The technical solution of this embodiment is basically the same as that of the first embodiment, except that 0.5% FFA degassing penetrant and 1.5% Abaige B leveling agent are added in step S2; 1.5% soda ash is added in step S4; 0.5% formic acid and 0.5% cashmere softening agent are added in step S5. The components in this embodiment are relatively moderate.

[0037] Embodiment three:

[0038] The technical solution of this embodiment is basically the same as that of the first embodiment, except that 0.55% FFA degassing penetrant and 1.55% Abaige B leveling agent are added in step S2; 1.55% soda ash is added in step S4; 0.55% formic acid and 0.55% cashmere softening agent are added in step S5. The components in this embodiment are higher.

[0039] The dyeing performance of the above three embodiments was tested, and the results are shown in Table 1:

[0040] Table 1

[0041]

[0042]

[0043] It can be seen from Table 1 that the dyeing method of the present invention can achieve good coloring effect of white velvet; good color fastness, significantly enhanced washing resistance, not easy to fade; and good softness, improving the feel of white velvet; among them, the dyeing rate of Example 2 is the best, the proportion of each group is the most reasonable, and the effect is the best.

[0044] The above-mentioned implementation modes are only preferred implementation modes of the present application and cannot be used to limit the scope of protection of the present application. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present application shall fall within the scope of protection required by the present application.

Claims

1. A method for dyeing white velvet into olive green using lanner dye, characterized in that: The following steps are involved: S1: Add white wool and dye solution into the dye vat, with the dye solution ratio being 1:15; S2: Heat to 40°C, add 0.45-0.55% FFA degassing penetrant and 1.45-1.55% Abaige B leveling agent based on the mass of white wool, add olive green lanner dye after 5 minutes, and maintain for 10 minutes; S3: Raise the temperature to 70°C at a rate of 1°C / 1.5 minutes. After 20 minutes, raise the temperature to 95°C at a rate of 1°C / 1 minute and maintain for 40 minutes. S4: Cool down to 80°C, add 1.45-1.55% soda ash based on the mass of the white wool, keep it for 20 minutes, then wash it with water and lower the temperature to 40°C; S5: Based on the quality of white cashmere, add 0.45-0.55% formic acid and 0.45-0.55% cashmere softener. After 20 minutes, the dyeing is completed.

2. The method for dyeing white velvet into olive green using lanner dye according to claim 1, characterized in that: In step S2, based on the mass of white wool, the olive green lanner dye is 1% CN dye, 1.19% lanner gold CE, 0.45% lanner red CE and 0.83% lanner blue CE.

3. The method for dyeing white velvet into olive green using lanner dye according to claim 2, characterized in that: The CN dye contains 25-30% of ethoxylated iso-rich C9-11 alcohol, 20-25% of ethoxylated tridecanol, 3-10% of oligomeric D-pyranose C10-16-alkyl glycoside, and the remainder is water.

4. The method for dyeing white velvet into olive green using lanner dye according to claim 1, characterized in that: In step S4, the washing is first performed twice with water at 60° C., and then twice with water at room temperature.

5. The method for dyeing white velvet into olive green using lanner dye according to claim 1, characterized in that: The cashmere softening agent in step S5 contains 4% ethoxylated isotriacontanol, 1% diethylene glycol butyl ether, 10% silicone oil, 0.2% acetic acid, and the remainder is water.

6. The method for dyeing white velvet into olive green using lanner dye according to claim 1, characterized in that: In the step S2, 0.45% FFA degassing penetrant and 1.45% Abaige B leveling agent are added; in the step S4, 1.45% soda ash is added; and in the step S5, 0.45% formic acid and 0.45% cashmere softening agent are added.

7. The method for dyeing white velvet into olive green using lanner dye according to claim 1, characterized in that: In the step S2, 0.5% FFA degassing penetrant and 1.5% Abaige B leveling agent are added; in the step S4, 1.5% soda ash is added; and in the step S5, 0.5% formic acid and 0.5% cashmere softening agent are added.

8. The method for dyeing white velvet into olive green using lanner dye according to claim 1, characterized in that: In the step S2, 0.55% FFA degassing penetrant and 1.55% Abaige B leveling agent are added; in the step S4, 1.55% soda ash is added; and in the step S5, 0.55% formic acid and 0.55% cashmere softening agent are added.