Meta-aramid paper as well as preparation method and application thereof
By using oxidation additives and wood pulp in meta-aramid paper, the rapid degradation of the material and excellent mechanical properties are achieved, and the problem of difficult degradation of existing meta-aramid paper is solved, which improves its high temperature and harshness Performance stability in the environment.
Patent Information
- Application Number
- CN202411062073.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The existing meta-aramid paper is difficult to degrade in the natural environment, resulting in ecological environment pollution, and its production cost is high, making it difficult to achieve both degradability and excellent mechanical properties.
The combination of oxidation additives and wood pulp is used to reduce the molecular weight of the polymer through preoxidation treatment and microbial decomposition, promote the rapid degradation of meta-aramid paper, and improve its mechanical properties and processing properties.
The rapid degradation and excellent mechanical properties of meta-aramid paper were achieved, with a degradation conversion rate of 26.2%. At the same time, the material performance was maintained in high temperature and harsh environments, and the weight and dielectric strength reached 39.9-40.9g/m2 and 14.2. kV/mm.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of papermaking, and in particular to meta-aramid paper and a preparation method and application thereof. Background Art
[0002] Meta-aramid paper (polyisophthalamide cellulose paper) is a new type of material. It is made of meta-aramid precipitated fibers and meta-aramid staple fibers through an inclined wire paper machine and hot-pressed at high temperature. It has high chemical and physical stability, acid and alkali corrosion resistance, flame retardancy and high temperature resistance, crack resistance and impact resistance, small wear deformation, good insulation, and long service life. It is widely used all over the world and is growing year by year. With the rapid development of high-speed trains, subways and light rails and the transformation of power grids, the demand for meta-aramid paper in traditional fields such as locomotive high-power traction transformers, motors and new power transmission and transformation equipment for smart grids has maintained steady growth. Emerging application fields of meta-aramid paper such as new energy vehicles, wind power generation, and domestic aircraft have gradually expanded, and the market demand for meta-aramid paper has gradually increased, with broad market development prospects. Data shows that the market size of my country's meta-aramid paper industry will reach US$226 million in 2022. Due to strong demand from downstream industries, China's consumption of meta-aramid paper reached 4,215 tons in 2021, with an average growth rate of 13.43% from 2017 to 2021.
[0003] At present, the main purpose of the research on meta-aramid paper is to improve its strength, corrosion resistance, high temperature resistance and other properties. For example, CN111668425A discloses a method for preparing a meta-aramid diaphragm, comprising the following steps: reacting meta-phenylenediamine, isophthaloyl chloride and calcium hydroxide in dimethylacetamide to obtain a meta-aramid solution; mixing the meta-aramid solution with dimethyl carbonate and adjusting the viscosity to 25000-30000 mPa.s to obtain a meta-aramid slurry; extruding the meta-aramid slurry to obtain a casting sheet, and stretching the casting sheet transversely to obtain a diaphragm precursor; stretching the diaphragm precursor vertically to obtain a diaphragm semi-finished product; extracting and curing the diaphragm semi-finished product, drying and rolling it to obtain a meta-aramid diaphragm. The present invention adds a considerable amount of calcium hydroxide during the synthesis process of meta-aramid to form a calcium salt system in the meta-aramid solution, thereby increasing the molecular weight of the meta-aramid and the viscosity and toughness of its slurry; during the film-making process, transverse and vertical stretching is performed to make the slurry form a film uniformly, reduce the internal stress during extraction and curing, make the pores inside the membrane uniform, and significantly improve the high temperature resistance of the diaphragm.
[0004] However, with the large-scale application of plastics, a large number of discarded plastic products can be seen everywhere in various public places. They come from industry, are made by humans, and are not easily absorbed by nature when they are finally returned to nature, thus affecting the ecological environment of nature. From the perspective of saving resources, since the main source of plastic products is the depleted oil resources, they should be recycled as much as possible, but since the current production cost of recycling is much higher than the direct production cost, it is difficult to do so under the current market economic conditions. Faced with the pollution problem, people hope to find a substitute that has the excellent performance of meta-aramid without causing white pollution.
[0005] Therefore, how to prepare meta-aramid with both excellent mechanical properties and degradable properties has become a problem that needs to be solved urgently. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a meta-aramid paper and a preparation method and application thereof. The raw materials for preparing the meta-aramid paper include a combination of meta-aramid fibrils, meta-aramid staple fibers, wood pulp and an oxidizing agent. The mechanical properties and processing properties of the meta-aramid material are improved by pre-oxidation with an oxidizing agent. At the same time, with the use of wood pulp, the rapid degradation of the meta-aramid paper in the soil is achieved, thereby obtaining meta-aramid paper with excellent mechanical properties and degradability.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a meta-aramid paper, wherein the raw materials for preparing the meta-aramid paper include a combination of meta-aramid fibrids, meta-aramid staple fibers, wood pulp and an oxidizing agent.
[0009] The meta-aramid paper provided by the present invention is a degradable meta-aramid, which is characterized in that after reaching a certain service life and being discarded, under specific environmental conditions, its chemical structure undergoes obvious changes, causing certain performance losses and appearance changes, and degrading, and is harmless or less harmful to the natural environment.
[0010] The reason why most plastic products (such as meta-aramid, polyethylene, polypropylene, etc.) are not easily biodegradable in the natural environment is that the huge molecular structure of these artificial polymers (molar mass of about 250,000) inhibits the ability of microorganisms in nature to digest them as a carbon source. Therefore, in order to make the macromolecules in artificial polymers biodegraded by biotransformation, first of all, we must try to reduce their molecular weight to the level of chemicals in nature (molar mass of about 5,000-10,000). This goal can be achieved through the "Norish" chemical reaction, that is, the contact reaction with certain metal ions. As the molecular weight of the polymer decreases, the polymer begins to become brittle and fragile. When the molecular weight is reduced to 10,000, it is easy to be eroded by natural microorganisms such as bacteria and fungi. At this time, if a hotbed suitable for the large-scale growth of microorganisms (such as cellulose) can be provided, the process of microbial engulfment, digestion and conversion begins. This natural decomposition process gradually transforms the polymer with reduced molecular weight into biomass until it is completely transformed into carbon dioxide, water and biomass.
[0011] The present invention is based on the understanding of this principle, and introduces two key substances that promote degradation into the meta-aramid: one is wood pulp with natural plant cellulose as the main component, which absorbs and aggregates microorganisms; the other is a pre-degradation component oxidation aid composed of some non-toxic non-heavy metal ions, and the degradation purpose is achieved through the synergistic effect of the two. After the meta-aramid is pre-oxidized by using the oxidation aid, the wood pulp is introduced into the meta-aramid. During the degradation process, the wood pulp contained in it is firstly rapidly decomposed by the enzymes secreted by microorganisms in the soil in a short time to generate cavities, resulting in the decrease of the mechanical properties of the meta-aramid paper. At the same time, the oxidation aid reacts with the metal salts in the soil to generate peroxides, which breaks the chain of the meta-aramid, and then degrades into small fragments that are easily devoured by microorganisms; then, various microorganisms and fungi are bred through the plant cellulose in the wood pulp, and rapidly multiply inside and outside the meta-aramid paper. During the process of reproduction and growth, these microorganisms continuously gnaw the meta-aramid paper into smaller and smaller pieces, and finally convert them into carbon dioxide, water and biomass, and at the same time play the role of improving the soil.
[0012] At the same time, the addition of the oxidation aid in the present invention can significantly improve the mechanical properties and processing properties of the meta-aramid material. The meta-aramid material after the composite oxidation aid has better thermal stability and chemical resistance, and can maintain the material's performance stability under high temperature and harsh environment. In addition, the use of the oxidation aid for pre-oxidation can also improve the interface compatibility of the meta-aramid material, so that it can be better combined with other materials, enhance the comprehensive performance of the material, and make up for the reduction in the mechanical properties of the meta-aramid paper caused by the introduction of wood pulp.
[0013] Preferably, in parts by weight, the preparation raw materials include 20-60 parts of meta-aramid fibrils (for example, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, etc.), 40-60 parts of meta-aramid staple fibers (for example, 42 parts, 45 parts, 48 parts, 50 parts, 52 parts, 55 parts, 58 parts, etc.), 2-20 parts of wood pulp (for example, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, etc.) and 0.1-1 part of an oxidizing agent (for example, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, etc.).
[0014] Preferably, in parts by weight, the preparation raw materials include 28-54 parts of meta-aramid fibrils (for example, 32 parts, 35 parts, 38 parts, 40 parts, 42 parts, 45 parts, 48 parts, 52 parts, etc.), 40-60 parts of meta-aramid staple fibers (for example, 42 parts, 45 parts, 48 parts, 50 parts, 52 parts, 55 parts, 58 parts, etc.), 4-18 parts of wood pulp (for example, 5 parts, 7 parts, 9 parts, 11 parts, 13 parts, 15 parts, 17 parts, etc.) and 0.2-0.6 parts of an oxidizing agent (for example, 0.25 parts, 0.35 parts, 0.45 parts, 0.55 parts, etc.).
[0015] Preferably, the density of the meta-aramid fibrid is 1.3-1.5 g / cm 3 , for example, 1.32 g / cm 3 , 1.35g / cm 3 , 1.38g / cm 3 , 1.4g / cm 3 , 1.42g / cm 3 , 1.45g / cm 3 , 1.48g / cm 3 wait.
[0016] Preferably, the length of the meta-aramid fibrid is 0.5-2 mm, for example, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm, 1.5 mm, 1.8 mm, etc.
[0017] Preferably, the meta-aramid fiber precipitation has a specific surface area of 40-80m 2 / g, for example, 45m 2 / g, 50m 2 / g, 55m 2 / g, 60m 2 / g, 65m 2 / g, 70m 2 / g, 75m 2 / g, etc.
[0018] Exemplarily, the meta-aramid fibrid is prepared by the following method:
[0019] (1) Preparation of polymer stock solution: m-phenylenediamine and isophthaloyl chloride are subjected to a low-temperature polycondensation reaction in an equal molar ratio to obtain a m-aramid resin solution, which is diluted with N,N-dimethylacetamide (DMAC) and neutralized with hydroxide, and then stirred and dispersed uniformly to obtain a polymer stock solution with a solid content of 11-15%;
[0020] (2) Preparation of precipitating agent: prepare a solution with a mass ratio of DMAC to deionized water of (20-50):(50-70), and stir evenly;
[0021] (3) Preparation of meta-aramid fibrids: The polymer stock solution and the precipitating agent are transported to a precipitator at a mass ratio of 1:(8-15) for high-speed shearing at a shear rate of 1500-3000 rpm, and the obtained fibrids are subjected to two-stage countercurrent water washing to obtain the fibrids.
[0022] The temperature of the low-temperature polycondensation is 0-8°C, for example, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, etc.
[0023] The solid content of the polymer stock solution is 11-15%, for example, it can be 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, etc.
[0024] The mass ratio of DMAC to deionized water is (20-50):(50-70), for example, it can be 20:60, 30:50, 30:60, 30:70, 40:50, 40:60, 40:70, 50:60, etc.
[0025] The mass ratio of the polymer stock solution to the precipitating agent is 1:(8-15), for example, it can be 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, etc.
[0026] The shearing speed is 1500-3000 rpm, for example, it can be 1600 rpm, 1800 rpm, 2000 rpm, 2200 rpm, 2400 rpm, 2600 rpm, 2800 rpm, etc.
[0027] Preferably, the linear density of the meta-aramid staple fiber is 1.5-2D, for example, 1.6D, 1.7D, 1.8D, 1.9D, etc.
[0028] Preferably, the length of the meta-aramid staple fiber is 6-8 mm, for example, it may be 6.2 mm, 6.5 mm, 6.8 mm, 7 mm, 7.2 mm, 7.5 mm, 7.8 mm, etc.
[0029] Exemplarily, the meta-aramid staple fiber can be prepared by the following method:
[0030] (1) conducting a low-temperature polycondensation reaction of m-phenylenediamine and isophthaloyl chloride in an equal molar ratio to obtain a m-aramid resin solution, diluting it with N,N-dimethylacetamide (DMAC) and neutralizing it with hydroxide, and then stirring and dispersing it uniformly to obtain a polymer stock solution with a solid content of 16-20%;
[0031] (2) After degassing and filtration, the polymer stock solution obtained in step (1) enters a primary coagulation bath through a spinneret to obtain primary fibers, and then passes through a secondary coagulation bath, hot water drawing, water washing, drying, dry heat drawing, and heat setting to obtain aramid meta-aramid fiber filaments, and then passes through a fiber cutting machine to cut meta-aramid staple fibers with a length of 6-8 mm.
[0032] The solid content of the polymer stock solution is 16-20%, for example, it can be 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, etc.
[0033] Preferably, the wood pulp includes kraft wood pulp and / or sulfite wood pulp, and more preferably kraft wood pulp.
[0034] Preferably, the solid content of the wood pulp is 30-40%, for example, it can be 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% and the like.
[0035] Preferably, the fiber length of the wood pulp is 0.7-0.8 mm, for example, it can be 0.72 mm, 0.74 mm, 0.76 mm, 0.78 mm, etc.
[0036] Preferably, the fiber thickness of the wood pulp is 0.05-0.06 mg / m, for example, it can be 0.052 mg / m, 0.054 mg / m, 0.056 mg / m, 0.058 mg / m, etc.
[0037] Preferably, the fiber quantity of the wood pulp is 12.5-14.0 million / g, for example, it can be 12.6 million / g, 12.8 million / g, 13 million / g, 13.2 million / g, 13.5 million / g, 13.8 million / g, etc.
[0038] Preferably, the oxidation aid includes any one of peroxide, unsaturated fatty acid or potassium permanganate, or a combination of at least two thereof.
[0039] The oxidizing aid in the present invention is a substance that can react with a metal salt to generate a peroxide. The generated peroxide can cut the polymer molecular chain, increase the surface area of the polymer, and then synergize with the cellulose-containing wood pulp to complete the rapid degradation of the meta-aramid paper, which is safe, green and environmentally friendly.
[0040] Preferably, the peroxide comprises hydrogen peroxide.
[0041] Preferably, the unsaturated fatty acid includes any one of oleic acid, linoleic acid, linolenic acid or arachidonic acid, or a combination of at least two thereof.
[0042] In a second aspect, the present invention provides a method for preparing the meta-aramid paper according to the first aspect, the preparation method comprising the following steps:
[0043] The meta-aramid fibrid, meta-aramid staple fibers, wood pulp and an oxidizing agent are mixed and then formed into a sheet to obtain the meta-aramid paper.
[0044] Preferably, the preparation method comprises the following steps:
[0045] (1) mixing an oxidizing agent with meta-aramid fibrid to obtain pre-oxidized meta-aramid fibrid;
[0046] (2) mixing the pre-oxidized meta-aramid fibrid obtained in step (1) with wood pulp to obtain mixed meta-aramid fibrid;
[0047] (3) Mixing the mixed meta-aramid fibrid obtained in step (2) with meta-aramid staple fibers and water to obtain a meta-aramid fiber suspension, and forming the suspension into a sheet to obtain the meta-aramid paper.
[0048] Preferably, the mass ratio of the oxidizing agent to the meta-aramid fibrid in step (1) is 1:(80-120), for example, it can be 1:85, 1:90, 1:95, 1:100, 1:105, 1:110, 1:115, etc.
[0049] Preferably, the mixing temperature in step (1) is 10-20°C, for example, it can be 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, etc.
[0050] Preferably, the mixing time in step (1) is 10-90 min, for example, 15 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, etc.
[0051] Preferably, the mixing in step (1) comprises stirring and / or ultrasonic dispersion.
[0052] Preferably, the frequency of the ultrasonic dispersion is 80-120 KHz, for example, 85 KHz, 90 KHz, 95 KHz, 100 KHz, 105 KHz, 110 KHz, 115 KHz, etc.
[0053] Preferably, the power of the ultrasonic dispersion is 1000-1500 W, for example, 1050 W, 1100 W, 1150 W, 1200 W, 1250 W, 1300 W, 1350 W, 1400 W, 1450 W, etc.
[0054] Preferably, the mixing in step (1) is followed by filtering.
[0055] Preferably, in parts by weight, the mixed meta-aramid fibrid comprises 70-90 parts (for example, 72 parts, 75 parts, 78 parts, 80 parts, 82 parts, 85 parts, 88 parts, etc.) of pre-oxidized meta-aramid fibrid and 10-30 parts (for example, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts, etc.) of wood pulp.
[0056] Preferably, the specific surface area of the mixed meta-aramid fiber is 40-70 m 2 / g, for example, 45m 2 / g, 50m 2 / g, 55m 2 / g, 60m 2 / g, 65m 2 / g, etc.
[0057] Preferably, the density of the mixed meta-aramid fibrid is 1.0-1.5 g / cm 3 , for example, it can be 1.1 g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 wait.
[0058] Preferably, the length of the mixed meta-aramid fibrid is 0.5-4 mm, for example, 0.8 mm, 1 mm, 1.2 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, etc.
[0059] Preferably, the mixing temperature in step (2) is 0-10°C, for example, it can be 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, etc.
[0060] Preferably, the mixing time in step (2) is 30-90 min, for example, it can be 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, etc.
[0061] Preferably, the mass ratio of the mixed meta-aramid fibrid to the meta-aramid staple fibers in step (3) is 1:(0.67-1.5), for example, it can be 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, etc.
[0062] Preferably, the water in step (3) is deionized water.
[0063] Preferably, the mixing temperature in step (3) is 15-30°C, for example, 18°C, 20°C, 22°C, 25°C, 28°C, etc.
[0064] Preferably, the mixing time in step (3) is 10-60 min, for example, it can be 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, etc.
[0065] Preferably, the mixing speed in step (3) is 1000-2000 r / min, for example, it can be 1100 r / min, 1200 r / min, 1300 r / min, 1400 r / min, 1500 r / min, 1600 r / min, 1700 r / min, 1800 r / min, 1900 r / min, etc.
[0066] Preferably, in the meta-aramid fiber suspension, the total concentration of mixed meta-aramid fibrids and meta-aramid staple fibers is 0.01-0.1wt%, for example, it can be 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, etc.
[0067] Preferably, the papermaking and forming operation includes using a paper machine to make paper, and then using a calender to calender the paper after drying.
[0068] Preferably, the paper machine comprises a tilted wire paper machine.
[0069] Preferably, the drying temperature is 70-95°C, for example, it can be 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, etc.
[0070] Preferably, the drying time is 60-120 s, for example, 70 s, 80 s, 90 s, 100 s, 110 s, etc.
[0071] Preferably, the drying comprises vacuum drying.
[0072] Preferably, the calender comprises a roll calender.
[0073] Preferably, the calendering temperature is 270-300°C, for example, 275°C, 280°C, 285°C, 290°C, 295°C, etc.
[0074] Preferably, the calendering pressure is 8-12 MPa, for example, it may be 8.5 MPa, 9 MPa, 9.5 MPa, 10 MPa, 10.5 MPa, 11 MPa, 11.5 MPa, etc.
[0075] Preferably, the calendering speed is 8-15 m / min, for example, it can be 8.5 m / min, 9 m / min, 9.5 m / min, 10 m / min, 10.5 m / min, 11 m / min, 11.5 m / min, 12 m / min, 13 m / min, 14 m / min, etc.
[0076] Preferably, the preparation method comprises the following steps:
[0077] (1) mixing an oxidizing agent and meta-aramid fibrid at 10-20° C. for 10-90 min, filtering, and obtaining pre-oxidized meta-aramid fibrid, wherein the mass ratio of the oxidizing agent to the meta-aramid fibrid is 1:(80-120);
[0078] (2) mixing 70-90 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 10-30 parts of wood pulp at 0-10° C. for 30-90 minutes to obtain mixed meta-aramid fibrids;
[0079] (3) mixing the mixed meta-aramid fibrid obtained in step (2) with meta-aramid staple fibers and water to obtain a meta-aramid fiber suspension, wherein the total concentration of the mixed meta-aramid fibrid and the meta-aramid staple fibers is 0.01-0.1 wt %, and papermaking is performed using a paper machine, and after drying at 70-95° C., calendering is performed using a calender at 270-300° C., 8-12 MPa, and 8-15 m / min to obtain the meta-aramid paper;
[0080] Wherein, the mass ratio of the mixed meta-aramid fibrid to the meta-aramid staple fiber is 1:(0.67-1.5).
[0081] In the preparation method of meta-aramid paper provided by the present invention, firstly, meta-aramid fibrid is modified with an oxidation aid to obtain pre-oxidized fibrid, and then mixed with wood pulp to form mixed meta-aramid fibrid for papermaking, which is used for filling and bonding of paper, and then mixed with meta-aramid staple fibers, and dispersed with water to form a low-concentration fiber aqueous solution to achieve structural enhancement of paper. In the papermaking process, the present invention adopts mixed meta-aramid fibrid and meta-aramid staple fibers to improve the overall bonding stability of meta-aramid base paper, and compared with traditional pure meta-aramid paper, it has excellent mechanical properties and degradability.
[0082] In a third aspect, the present invention provides a use of the meta-aramid paper as described in the first aspect in construction, electronics, automobiles, aircraft or power generation.
[0083] Compared with the prior art, the present invention has at least the following beneficial effects:
[0084] The invention provides a meta-aramid paper. The raw materials for preparing the meta-aramid paper include a combination of meta-aramid fibrillation, meta-aramid staple fibers, wood pulp and an oxidizing agent. By adding the oxidizing agent and the wood pulp, the two synergistically achieve rapid degradation of the meta-aramid paper and improve its mechanical properties. The prepared meta-aramid paper has a thickness of 0.05-0.052 mm and a gram weight of 39.9-40.9 g / m 2 , longitudinal tensile strength ≥4.18kN / m, transverse tensile strength ≥2.04kN / m, dielectric strength ≥14.2kV / mm, degradation conversion rate ≥26.2%. DETAILED DESCRIPTION
[0085] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0086] In the following specific implementation of the present invention, the materials involved are as follows:
[0087] 1. Meta-aramid fiber precipitation
[0088] (1) Preparation of polymer stock solution: m-phenylenediamine and isophthaloyl chloride in equal molar ratios are subjected to polycondensation reaction at 4° C. to obtain a m-aramid resin solution, which is diluted with DMAC and neutralized with hydroxide, and then stirred and dispersed uniformly to obtain a polymer stock solution with a solid content of 13%;
[0089] (2) Preparation of precipitating agent: prepare a solution with a mass ratio of DMAC to deionized water of 30:70 and stir evenly;
[0090] (3) Preparation of meta-aramid fibrids: The polymer stock solution and the precipitating agent were transported to a precipitator at a mass ratio of 1:10 for high-speed shearing at a shear rate of 2000 rpm, and the obtained fibrids were subjected to two-stage countercurrent water washing to obtain the fibrids.
[0091] 2. Meta-aramid staple fiber
[0092] (1) carrying out polycondensation reaction of m-phenylenediamine and isophthaloyl chloride in equal molar ratio at 4° C. to obtain a m-aramid resin solution, which is diluted with DMAC and neutralized with hydroxide, and then stirred and dispersed uniformly to obtain a polymer stock solution with a solid content of 18%;
[0093] (2) After degassing and filtration, the polymer solution obtained in step (1) enters a primary coagulation bath through a spinneret to obtain primary fibers, and then passes through a secondary coagulation bath, hot water drawing, water washing, drying, dry heat drawing, and heat setting to obtain aramid meta-aramid fiber filaments, and then passes through a fiber cutting machine to cut meta-aramid staple fibers of 6 mm in length.
[0094] 3. Wood pulp
[0095] Asia Pacific Sembo (Shandong) Pulp and Paper Co., Ltd., Model: Specialty Paper Pulp (BPSP Pulp), Fiber Length: 0.7-0.8mm, Fiber Coarseness: 0.05-0.06mg / m, Fiber Quantity: 12.5-14.0million / g
[0096] 4. Pregelatinized starch
[0097] Langfang Changlin Cellulose Co., Ltd., Model: CLHG-002, Fineness: 80 mesh, Purity: 99.9%, Density: 1.3g / m 3 , viscosity: greater than 300mpa·s
[0098] Example 1
[0099] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0100] (1) In an aramid fibrid storage tank equipped with a mechanical stirring device, an ultrasonic generator and automatic temperature control, hydrogen peroxide is placed in the storage tank at a mass ratio of 1:100, the storage tank temperature is set to 10° C., stirring and mixing, and ultrasonic dispersion at a working frequency of 100 KHz is used for 60 minutes. After standing, the mixture is filtered to obtain pre-oxidized meta-aramid fibrid containing hydrogen peroxide;
[0101] (2) mixing 70 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 30 parts of wood pulp at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0102] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1.5 and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min at room temperature for 30 min to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers, which is introduced into an inclined wire paper machine and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the mixture is calendered at 290° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0103] Example 2
[0104] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0105] (1) In an aramid fibrid storage tank equipped with a mechanical stirring device, an ultrasonic generator and automatic temperature control, hydrogen peroxide is placed in the storage tank at a mass ratio of 1:100, the storage tank temperature is set to 15° C., stirring and mixing, and simultaneously using an ultrasonic wave with a working frequency of 80 KHz for 60 minutes, and then standing and filtering to obtain pre-oxidized meta-aramid fibrid containing hydrogen peroxide;
[0106] (2) mixing 50 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 50 parts of wood pulp at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0107] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1.22, and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min at room temperature for 30 min to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers, which is introduced into an inclined wire paper machine and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the mixture is calendered at 290° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0108] Example 3
[0109] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0110] (1) In an aramid fibrid storage tank equipped with a mechanical stirring device, an ultrasonic generator and automatic temperature control, hydrogen peroxide is placed in the storage tank at a mass ratio of 1:100, the storage tank temperature is set to 10° C., stirring and mixing, and ultrasonic dispersion at a working frequency of 100 KHz is used for 60 minutes. After standing, the mixture is filtered to obtain pre-oxidized meta-aramid fibrid containing hydrogen peroxide;
[0111] (2) mixing 90 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 10 parts of wood pulp at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0112] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1 and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min for 30 min at room temperature to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers. The suspension is introduced into an inclined wire paper machine, and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the suspension is calendered at 290° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0113] Example 4
[0114] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0115] (1) In an aramid fibrid storage tank equipped with a mechanical stirring device, an ultrasonic generator and automatic temperature control, potassium permanganate is placed in the storage tank at a mass ratio of 1:100, the storage tank temperature is set to 10° C., the mixture is stirred and mixed, and ultrasonic dispersion is performed at a working frequency of 100 KHz for 60 minutes. After standing, the mixture is filtered to obtain pre-oxidized meta-aramid fibrid containing potassium permanganate;
[0116] (2) mixing 90 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 10 parts of wood pulp at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0117] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1 and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min for 30 min at room temperature to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers. The suspension is introduced into an inclined wire paper machine, and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the suspension is calendered at 290° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0118] Example 5
[0119] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0120] (1) In an aramid fibrid storage tank equipped with a mechanical stirring device, an ultrasonic generator and automatic temperature control, hydrogen peroxide is placed in the storage tank at a mass ratio of 1:121, the storage tank temperature is set at 10° C., stirred and mixed, and ultrasonic dispersion at a working frequency of 100 KHz is used for 60 minutes. After standing, the mixture is filtered to obtain pre-oxidized meta-aramid fibrid containing hydrogen peroxide;
[0121] (2) mixing 90 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 10 parts of wood pulp at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0122] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1 and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min for 30 min at room temperature to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers. The suspension is introduced into an inclined wire paper machine, and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the suspension is calendered at 290° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0123] Comparative Example 1
[0124] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0125] (1) mixing 90 parts of meta-aramid fibrids with 10 parts of wood pulp at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0126] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1 and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min at room temperature for 30 min to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers. The suspension is introduced into an inclined wire paper machine, and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the suspension is calendered at 280° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0127] Comparative Example 2
[0128] A meta-aramid paper, wherein the meta-aramid paper is prepared by the following method:
[0129] (1) In an aramid fibrid storage tank equipped with a mechanical stirring device, an ultrasonic generator and automatic temperature control, hydrogen peroxide is placed in the storage tank at a mass ratio of 1:100, the storage tank temperature is set to 10° C., stirring and mixing, and ultrasonic dispersion at a working frequency of 100 KHz is used for 60 minutes. After standing, the mixture is filtered to obtain pre-oxidized meta-aramid fibrid containing hydrogen peroxide;
[0130] (2) mixing 90 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 10 parts of pregelatinized starch at 0° C. for 90 minutes to obtain mixed meta-aramid fibrids;
[0131] (3) The mixed meta-aramid fibrids and meta-aramid staple fibers obtained in step (2) are mixed in a mixing tank at a mass ratio of 1:1 and then transferred to a storage tank, deionized water is added, and the mixture is stirred at 1500 r / min at room temperature for 30 min to obtain a meta-aramid fiber suspension with a total concentration of 0.04 wt% of the mixed meta-aramid fibrids and meta-aramid staple fibers. The suspension is introduced into an inclined wire paper machine, and papermaking is performed on the paper machine. After drying at 95° C. for 1 min, the suspension is calendered at 280° C. and 10 MPa at 10 m / min on a roller calender to obtain the meta-aramid paper.
[0132] Test Method
[0133] 1. Thickness
[0134] Reference national standard: GB / T 451.3-2002 Determination of thickness of paper and paperboard
[0135] 2. Weight
[0136] Reference national standard: GB / T 451.2-2002 Determination of the basis weight of paper and paperboard
[0137] 3. Tensile strength
[0138] Reference national standard: GB / T12914-2018 Determination of tensile strength of paper and paperboard
[0139] 4. Dielectric strength
[0140] Reference national standard: GB / T 1408.1-2006 Test method for electrical strength of insulating materials
[0141] 5. Degradation conversion rate
[0142] Reference national standard: GB / T41010-2021 Degradation performance and labeling of biodegradable plastics and products
[0143] Degradation conversion rate = (initial aramid paper amount - mass of the remaining solid after degradation after drying) / initial aramid paper amount * 100%.
[0144] The test results are shown in Table 1.
[0145] Table 1
[0146]
[0147] It can be seen from the test results of Examples 1-5 that the meta-aramid paper provided by the present invention achieves the degradation of the meta-aramid paper by adding an oxidizing agent and wood pulp, and at the same time improves its mechanical properties and electrical properties. The prepared meta-aramid paper has a thickness of 0.05-0.052 mm and a gram weight of 39.9-40.9 g / m 2 , longitudinal tensile strength ≥4.18kN / m, transverse tensile strength ≥2.04kN / m, dielectric strength ≥14.2kV / mm, degradation conversion rate ≥26.2%. It can be seen from Examples 3 to 5 that the present invention can achieve better technical effects of improving tensile strength, dielectric strength and degradation conversion rate by further replacing different oxidizing aids and adjusting the proportion of oxidizing aids.
[0148] It can be seen from Example 3 and Comparative Example 1 that the present invention can obtain the technical effect of high degradability by adopting an oxidizing agent, while when the oxidizing agent is lacking, it is impossible to obtain meta-aramid paper with excellent degradability.
[0149] It can be seen from Example 3 and Comparative Example 2 that the present invention can achieve the technical effect of comparing the absorption and growth of microorganisms of different materials by using gelatinized starch instead of wood pulp, while when wood pulp is not used, it cannot achieve the technical effect of excellent mechanical properties and degradable meta-aramid paper.
[0150] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A meta-aramid paper, characterized in that: The raw materials for preparing the meta-aramid paper include a combination of meta-aramid fibrids, meta-aramid staple fibers, wood pulp and an oxidizing agent.
2. The meta-aramid paper according to claim 1, characterized in that: In parts by weight, the raw materials for preparation include 20-60 parts of meta-aramid fibrids, 40-60 parts of meta-aramid staple fibers, 2-20 parts of wood pulp and 0.1-1 parts of an oxidizing agent; Preferably, in parts by weight, the raw materials for preparation include 28-54 parts of meta-aramid fibrids, 40-60 parts of meta-aramid staple fibers, 4-18 parts of wood pulp and 0.2-0.6 parts of an oxidizing agent.
3. The meta-aramid paper according to claim 1 or 2, characterized in that: The density of the meta-aramid fiber is 1.3-1.5 g / cm 3 ; Preferably, the length of the meta-aramid fibrid is 0.5-2 mm; Preferably, the meta-aramid fiber precipitation has a specific surface area of 40-80m 2 / g; Preferably, the linear density of the meta-aramid staple fiber is 1.5-2D; Preferably, the length of the meta-aramid staple fiber is 6-8 mm; Preferably, the wood pulp comprises kraft wood pulp and / or sulfite wood pulp; Preferably, the solid content of the wood pulp is 30-40%; Preferably, the fiber length of the wood pulp is 0.7-0.8 mm; Preferably, the fiber thickness of the wood pulp is 0.05-0.06 mg / m; Preferably, the fiber quantity of the wood pulp is 12.5-14.0 million / g; Preferably, the oxidizing aid comprises any one or a combination of at least two of peroxide, unsaturated fatty acid or potassium permanganate; Preferably, the peroxide comprises hydrogen peroxide; Preferably, the unsaturated fatty acid includes any one of oleic acid, linoleic acid, linolenic acid or arachidonic acid, or a combination of at least two thereof.
4. A method for preparing the meta-aramid paper according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: The meta-aramid fibrid, meta-aramid staple fibers, wood pulp and an oxidizing agent are mixed and then formed into sheets to obtain the meta-aramid paper.
5. The preparation method according to claim 4, characterized in that: The preparation method comprises the following steps: (1) mixing an oxidizing agent with meta-aramid fibrid to obtain pre-oxidized meta-aramid fibrid; (2) mixing the pre-oxidized meta-aramid fibrid obtained in step (1) with wood pulp to obtain mixed meta-aramid fibrid; (3) Mixing the mixed meta-aramid fibrid obtained in step (2) with meta-aramid staple fibers and water to obtain a meta-aramid fiber suspension, and forming the suspension into a sheet to obtain the meta-aramid paper.
6. The preparation method according to claim 5, characterized in that: The mass ratio of the oxidizing agent to the meta-aramid fiber precipitate in step (1) is 1:(80-120); Preferably, the mixing temperature in step (1) is 10-20°C; Preferably, the mixing time in step (1) is 10-90 min; Preferably, the mixing in step (1) comprises stirring and / or ultrasonic dispersion; Preferably, the frequency of the ultrasonic dispersion is 80-120 KHz; Preferably, the power of the ultrasonic dispersion is 1000-1500W; Preferably, the mixing in step (1) is followed by filtering.
7. The preparation method according to claim 5 or 6, characterized in that: In parts by weight, the mixed meta-aramid fibrid comprises 70-90 parts of pre-oxidized meta-aramid fibrid and 10-30 parts of wood pulp; Preferably, the specific surface area of the mixed meta-aramid fiber is 40-70 m 2 / g; Preferably, the density of the mixed meta-aramid fibrid is 1.0-1.5 g / cm 3 ; Preferably, the length of the mixed meta-aramid fibrid is 0.5-4 mm; Preferably, the mixing temperature in step (2) is 0-10°C; Preferably, the mixing time in step (2) is 30-90 min.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The mass ratio of the mixed meta-aramid fibrid to the meta-aramid staple fibers in step (3) is 1:(0.67-1.5); Preferably, the water in step (3) is deionized water; Preferably, the mixing temperature in step (3) is 15-30°C; Preferably, the mixing time in step (3) is 10-60 min; Preferably, the mixing speed in step (3) is 1000-2000 r / min; Preferably, in the meta-aramid fiber suspension, the total concentration of mixed meta-aramid fibrids and meta-aramid staple fibers is 0.01-0.1 wt %; Preferably, the papermaking and forming operation includes using a paper machine to make paper, and using a calender to calender after drying; Preferably, the paper machine comprises an inclined wire paper machine; Preferably, the drying temperature is 70-95°C; Preferably, the drying time is 60-120s; Preferably, the drying comprises vacuum drying; Preferably, the calender comprises a roller calender; Preferably, the calendering temperature is 270-300°C; Preferably, the calendering pressure is 8-12 MPa; Preferably, the calendering speed is 8-15 m / min.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: (1) mixing an oxidizing agent and meta-aramid fibrid at 10-20° C. for 10-90 min, filtering, and obtaining pre-oxidized meta-aramid fibrid, wherein the mass ratio of the oxidizing agent to the meta-aramid fibrid is 1:(80-120); (2) mixing 70-90 parts of the pre-oxidized meta-aramid fibrids obtained in step (1) with 10-30 parts of wood pulp at 0-10° C. for 30-90 minutes to obtain mixed meta-aramid fibrids; (3) mixing the mixed meta-aramid fibrid obtained in step (2) with meta-aramid staple fibers and water to obtain a meta-aramid fiber suspension, wherein the total concentration of the mixed meta-aramid fibrid and the meta-aramid staple fibers is 0.01-0.1 wt %, and papermaking is performed using a paper machine. After drying, calendering is performed using a calender at 270-300° C., 8-12 MPa, and 8-15 m / min to obtain the meta-aramid paper; Wherein, the mass ratio of the mixed meta-aramid fibrid to the meta-aramid staple fiber is 1:(0.67-1.5).
10. Use of the meta-aramid paper according to any one of claims 1 to 3 in construction, electronics, automobiles, aircraft or power generation.
Citation Information
Patent Citations
Method for improving aramid surface activity
CN104264451A
Composite plant fiber aramid paper and preparation method thereof
CN105648830A