Flexible tactile sensing array and preparation method thereof

By setting the arrayed ionic dielectric layer and raised microstructure in the tactile sensing array, the problem of poor array crosstalk and preparation repeatability is solved, and high sensitivity and high interference resistance is achieved, and it is suitable for fields such as intelligent robots and intelligent medical care.

CN118980443APending Publication Date: 2024-11-19JIASHAN FUDAN RESEARCH INSTITUTE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310582363.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The tactile sensing array based on the electric double layer effect has problems such as serious array crosstalk and poor preparation repeatability, which cannot meet the practical application needs.

Method used

Using an arrayed ion dielectric layer, by providing an arrayed ion dielectric layer between the first array electrode and the second array electrode, the dielectric layer includes a planar structure with a sensing site close to the first array electrode and a convex adjacent to the second array electrode. The microstructure is formed and the pores are filled with polydimethylsiloxane film and ionic polymer gel layer to form a raised microstructure, reducing array crosstalk and improving sensitivity.

Benefits of technology

High sensitivity, low array crosstalk, high anti-interference and good stability are achieved, and the preparation method is easy to achieve and large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980443A_ABST
    Figure CN118980443A_ABST
Patent Text Reader

Abstract

The invention provides a flexible tactile sensing array and a preparation method thereof. The flexible tactile sensing array comprises a first array electrode and a second array electrode which are oppositely arranged, the array ionic medium layer is arranged between the first array electrode and the second array electrode; the arrayed ionic dielectric layer comprises a plurality of sensing sites arranged in an array mode, the side face, close to the first array electrode, of each sensing site is of a plane structure, and the side face, close to the second array electrode, of each sensing site is of a protruding microstructure. The flexible tactile sensing array and the preparation method thereof provided by the invention have the advantages of high sensitivity, low array crosstalk, high anti-interference performance and good stability, and the preparation method is high in repeatability and easy to implement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sensor technology, and in particular to a flexible tactile sensor array and a preparation method thereof. Background Art

[0002] With the rapid development of robotics and artificial intelligence, people are increasingly in need of flexible wearable devices that can sense various information in the environment and use them in fields such as intelligent robots and intelligent medical care. In recent years, tactile sensors based on the electric double layer (EDL) effect have become a research hotspot due to their excellent performance. Its working principle is to use electrodes and ionic dielectric layers to form a nanoscale ion-electron double layer interface, which can greatly increase the capacitance value of capacitive sensors. The initial capacitance value of sensor devices based on the double layer effect is thousands of times higher than that of traditional parallel plate capacitors of the same size. Therefore, it can significantly reduce the interference of human body capacitive noise and parasitic capacitance on the real sensing signal and improve the signal-to-noise ratio of the sensor. At the same time, a small change in external stress can result in a large change in capacitance value, thus having the characteristics of ultra-high sensitivity.

[0003] Generally, tactile sensor arrays based on the double-layer effect only process the electrodes in an array, and the ionic dielectric layer is an integrated structure. According to the sensing principle, the migration of ions can occur in the entire dielectric layer, so in this case, more serious crosstalk will be formed between the sensing array sites.

[0004] At the same time, the microstructure on the surface of the ionic dielectric layer can effectively improve the sensitivity of the tactile sensor device. Generally, an irregular convex structure is obtained by using a sandpaper template or paper; or an irregular nanofiber structure is obtained by electrospinning. The above preparation methods all have problems such as irregular structure, poor repeatability, and inability to prepare on a large scale, which cannot meet the actual application requirements. Summary of the invention

[0005] The object of the present invention is to provide a flexible tactile sensor array and a preparation method thereof, which has high sensitivity, low array crosstalk, high anti-interference and good stability, and the preparation method has high repeatability and is easy to implement.

[0006] To achieve the above objectives, in a first aspect, the present invention provides a flexible tactile sensor array, comprising:

[0007] A first array electrode and a second array electrode arranged opposite to each other;

[0008] an arrayed ion medium layer disposed between the first array electrode and the second array electrode;

[0009] The arrayed ion medium layer includes a plurality of sensing sites arranged in an array. A side of the sensing site close to the first array electrode is a planar structure, and a side of the sensing site close to the second array electrode is a protruding microstructure.

[0010] In some embodiments, the arrayed ion medium layer includes a polydimethylsiloxane film with a plurality of array filling holes and a plurality of ion polymer gel layers;

[0011] A plurality of the ionic polymer gel layers are respectively filled in the filling holes to form the sensing sites.

[0012] In some embodiments, the raised microstructure includes any one of a pyramidal structure, a conical structure, and a columnar structure.

[0013] In a second aspect, the present invention provides a method for preparing a flexible tactile sensor array, which is used to prepare the flexible tactile sensor array, and the preparation method comprises:

[0014] forming a first array electrode and a second array electrode;

[0015] forming an arrayed ion medium layer;

[0016] The arrayed ion medium layer is attached between the first array electrode and the second array electrode to form the flexible tactile sensor array.

[0017] In some embodiments, forming the first array electrode and the second array electrode comprises:

[0018] providing a flexible substrate;

[0019] Disposing a flexible electrode material on the flexible substrate to form an array electrode;

[0020] The array electrode includes the first array electrode and the second array electrode.

[0021] In some embodiments, the flexible substrate is made of polydimethylsiloxane, and the thickness of the flexible substrate is 50-200 μm.

[0022] In some embodiments, the flexible electrode material includes any one of silver nanofibers, liquid metal, nanosheet ink, carbon nanotubes, and nanowires.

[0023] In some embodiments, the array electrodes are formed on the flexible substrate by using a laser marker, printing technology or inkjet printing technology.

[0024] In some embodiments, the forming of the arrayed ion medium layer comprises:

[0025] Providing a template with an array-distributed protrusion structure, each protrusion structure being provided with a plurality of groove microstructures;

[0026] Providing a polydimethylsiloxane film having a plurality of array-filled holes;

[0027] Laminating the polydimethylsiloxane film on the template, with the filling hole aligned with the protruding structure;

[0028] An ionic polymer gel layer is filled in the filling hole to form a sensing site.

[0029] In some embodiments, the plurality of groove microstructures include any one of a pyramidal structure, a conical structure, and a columnar structure.

[0030] In some embodiments, the step of filling the filling hole with an ionic polymer gel layer to form a sensing site comprises:

[0031] The ionic polymer gel solution is filled into the groove microstructure through the filling holes to form a protruding microstructure.

[0032] In some embodiments, before providing a polydimethylsiloxane film having a plurality of array-filled holes, the method comprises:

[0033] Cutting the polydimethylsiloxane isolation film with a laser to obtain the filling hole;

[0034] Treating the inner sidewalls of the filling holes with plasma to form dense active silicon-oxygen groups on the inner sidewalls of the filling holes;

[0035] placing the polydimethylsiloxane film treated with plasma into a prepared silane coupling agent solution for amination;

[0036] The aminated polydimethylsiloxane film is immersed in a glutaraldehyde mixed solution to cause a Schiff base synthesis reaction.

[0037] In some embodiments, treating the inner sidewall of the filling hole with plasma comprises:

[0038] The plasma processing power is set to 40-60W and the operation is continued for 30-60s.

[0039] In some embodiments, the silane coupling agent solution includes 3-aminopropyltriethoxysilane, ethanol and deionized water; wherein,

[0040] The volume fraction of 3-aminopropyltriethoxysilane in the silane coupling agent solution is 15% to 30%, the volume fraction of ethanol is 30% to 50%, and the volume fraction of deionized water is 30% to 50%.

[0041] In some embodiments, the volume fraction of the aqueous solution in the glutaraldehyde mixture is 2% to 10%, and the reaction temperature is 30°C to 50°C.

[0042] In some embodiments, the ionic polymer gel solution comprises polyvinyl alcohol, an ionic liquid and a solvent; wherein,

[0043] The mass ratio of the polyvinyl alcohol to the solvent is 1:8 to 1:12, and the mass ratio of the ionic liquid to the polyvinyl alcohol is 0.5:1 to 1:1.

[0044] The flexible tactile sensor array and the preparation method thereof provided by the present invention have the following beneficial effects:

[0045] 1. It has high sensitivity, low array crosstalk, high anti-interference and good stability.

[0046] 2. A good bonding force can be formed between the sensing site (ion gel) and the polydimethylsiloxane film, which greatly improves the robustness of the flexible tactile sensing array during application.

[0047] 3. The preparation method can be combined with inkjet printing technology, scraper technology, 3D printing template and laser marking technology, which has the advantages of easy implementation and large-scale preparation.

[0048] 4. Protruding microstructures are provided on the surface of the arrayed ion medium layer, which can effectively improve the sensitivity of the tactile sensor array. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 A three-dimensional diagram of a flexible tactile sensor array according to an embodiment of the present invention;

[0050] Figure 2 A side view of a flexible tactile sensor array according to an embodiment of the present invention;

[0051] Figure 3 A schematic diagram of the structure of an arrayed ion medium layer according to an embodiment of the present invention;

[0052] Figure 4 for Figure 3 Detailed view of point B in the middle;

[0053] Figure 5 A schematic diagram of the structure of a single tactile sensor device in an initial state and a state under pressure provided by an embodiment of the present invention;

[0054] Figure 6 An equivalent circuit diagram of a single flexible tactile device according to an embodiment of the present invention;

[0055] Figure 7A schematic diagram of the structure when an arrayed ion medium layer is formed in an embodiment provided by the present invention;

[0056] Figure 8 A flow chart of a method for preparing a flexible tactile sensor array according to an embodiment of the present invention;

[0057] Fig. 9 A flow chart of a method for preparing an arrayed ion medium layer according to an embodiment of the present invention;

[0058] Fig.10 for Figure 7 Detailed view of point A in the middle.

[0059] Reference numerals:

[0060] The first array electrode 1 , the second array electrode 2 , the arrayed ion medium layer 3 , the sensing site 31 , the protruding microstructure 32 , the polydimethylsiloxane film 33 , the filling hole 34 , the ion polymer gel layer 35 , the template 4 , and the groove microstructure 41 . DETAILED DESCRIPTION

[0061] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0062] Figure 1 A stereoscopic diagram of a flexible tactile sensor array according to an embodiment of the present invention. Figure 2 A side view of a flexible tactile sensor array according to an embodiment of the present invention.

[0063] refer to Figure 1 and Figure 2 As shown, an embodiment of the present invention provides a flexible tactile sensor array, comprising a first array electrode 1 and a second array electrode 2 arranged opposite to each other, and an arrayed ion medium layer 3 arranged between the first array electrode 1 and the second array electrode 2 .

[0064] Figure 3 This is a schematic diagram of the structure of the arrayed ion medium layer according to an embodiment of the present invention. Figure 4 for Figure 3 Detailed view of point B in the middle.

[0065] refer to Figure 3 and Figure 4 As shown, the arrayed ionic medium layer 3 includes a plurality of sensing sites 31 arranged in an array. Since the sensing sites 31 are arranged in an array, compared with the integrated structure of the medium layer in the prior art, the flexible tactile sensing array in this embodiment has low array crosstalk and high anti-interference performance.

[0066] Since the migration of ions may occur in the entire dielectric layer, in this case, the flexible tactile sensing array in this embodiment has low array crosstalk and high anti-interference performance by arranging the sensing sites 31 in an array.

[0067] In addition, the side of the sensing site 31 close to the first array electrode 1 is a planar structure, and the side of the sensing site 31 close to the second array electrode 2 is a protruding microstructure 32. The sensitivity of the flexible tactile sensor array can be effectively improved by providing the protruding microstructure 32.

[0068] Figure 5 A schematic diagram of the structure of a single flexible tactile sensor device in an initial state and a state under pressure provided by an embodiment of the present invention.

[0069] Figure 6 This is an equivalent circuit diagram of a single flexible tactile sensor device according to an embodiment of the present invention.

[0070] refer to Figures 1 to 6 As shown, in this embodiment, the first array electrode 1 is located above the second array electrode 2, and the first array electrode 1, the second array electrode 2 and the arrayed ion medium layer 3 form an ion-electron double layer at the interface. It can be regarded as that a C 上 A C is formed between the second array electrode 2 and the arrayed ion medium layer 3. 下 , C 上 and C 下 Due to the existence of the raised microstructure 32, the contact area between the second array electrode 2 and the arrayed ion medium layer 3 is much larger than the contact area between the first array electrode 1 and the arrayed ion medium layer 3, so the total capacitance C0≈C of the flexible tactile sensor device 上 , at the same time, C 上 The contact area (A) between the first array electrode 1 and the arrayed ion medium layer 3 0 ) is proportional to.

[0071] Therefore, when the outside world applies pressure to the flexible tactile sensor device ( Figure 3The downward direction of the right arrow in the figure indicates the direction of applied pressure), the contact area between the first array electrode 1 and the arrayed ion medium layer 3 becomes larger, and the contact area is (A') at this time. The double layer effect is enhanced, and the total capacitance value C' also increases accordingly, so the size of the external force can be sensed according to the value of the measured capacitance change.

[0072] Figure 7 A schematic diagram of the structure of an arrayed ion medium layer formed in an embodiment of the present invention.

[0073] refer to Figure 7 As shown, in some embodiments, the arrayed ionic medium layer 3 includes a polydimethylsiloxane film 33 with a plurality of array filling holes 34 and a plurality of ionic polymer gel layers 35. The plurality of ionic polymer gel layers 35 are respectively filled in the filling holes 34 to form the sensing sites 31.

[0074] Furthermore, the protruding microstructure 32 includes any one of a pyramid structure, a cone structure and a columnar structure.

[0075] In this embodiment, the protruding microstructures 32 are a plurality of conical structures.

[0076] Figure 8 The present invention provides a flowchart of a method for preparing a flexible tactile sensor array according to an embodiment of the present invention.

[0077] Fig. 9 This is a flow chart of a method for preparing an arrayed ion medium layer according to an embodiment of the present invention.

[0078] Fig.10 for Figure 7 Detailed view of point A in the middle.

[0079] refer to Figure 8 As shown, in another embodiment provided by the present invention, a method for preparing a flexible tactile sensor array is provided, and the preparation method is used to prepare the flexible tactile sensor array in the above embodiment, and the preparation method comprises:

[0080] S610: forming a first array electrode and a second array electrode.

[0081] In this step, the first array electrode and the second array electrode are specifically prepared as follows:

[0082] A flexible substrate is provided.

[0083] The flexible substrate may be a thin film made of polydimethylsiloxane, and the thickness of the flexible substrate is 50-200 μm.

[0084] In this embodiment, the thickness of the flexible substrate is 100 μm.

[0085] A flexible electrode material is arranged on the flexible substrate to form an array electrode.

[0086] In this embodiment, a laser marker, printing technology or inkjet printing technology can be used to directly obtain a patterned electrode on the flexible substrate.

[0087] In addition, the flexible electrode material may include any one of silver nanofibers, liquid metal, nanosheet ink, carbon nanotubes, and nanowires.

[0088] In this embodiment, two electrodes distributed vertically are used, so the array electrodes include the first array electrode and the second array electrode distributed vertically. It should be noted that the first array electrode and the second array electrode only indicate that the number of the array electrodes is two.

[0089] In some embodiments, the array electrodes may also be coplanar interdigitated electrodes, which will not be described in detail herein.

[0090] S620: forming an arrayed ion medium layer.

[0091] refer to Figure 7 and Fig. 9 As shown, the specific method for preparing the arrayed ion medium layer is as follows:

[0092] S621: providing a template having an array-distributed protrusion structure, each protrusion structure being provided with a plurality of groove microstructures.

[0093] In this step, the template 4 can be made of resin or polymethyl methacrylate.

[0094] Combination Figure 7 and Fig.10 As shown, in this step, the protruding structure on the template 4 may be provided with a groove microstructure 41 similar to a pyramid structure, a conical structure or a columnar microstructure.

[0095] S622: Provide a polydimethylsiloxane film 33 having a plurality of array filling holes 34.

[0096] In this step, the polydimethylsiloxane isolation film 33 may be cut by laser cutting to obtain a plurality of array filling holes 34 on the main body thereof.

[0097] Then, the inner sidewalls of the filling holes 34 are treated with plasma to form dense active silicon-oxygen groups on the inner sidewalls of the filling holes 34 .

[0098] The plasma may be oxygen plasma, and the processing power of the plasma is set to 40-60w, and the plasma continues to work for 30-60s.

[0099] In a specific implementation process, the plasma processing power can be set to 50w and continue to work for 45s.

[0100] Next, the polydimethylsiloxane film 33 treated with plasma is placed in a prepared silane coupling agent solution for amination.

[0101] It should be noted that the silane coupling agent solution may include 3-aminopropyltriethoxysilane, ethanol and deionized water. The volume fraction of 3-aminopropyltriethoxysilane in the silane coupling agent solution is 15% to 30%, the volume fraction of ethanol is 30% to 50%, and the volume fraction of deionized water is 30% to 50%.

[0102] Finally, the aminated polydimethylsiloxane film 33 is immersed in a glutaraldehyde mixed solution to cause a Schiff base synthesis reaction.

[0103] Specifically, the volume fraction of the aqueous solution in the glutaraldehyde mixture is 2% to 10%, and the reaction temperature during the Schiff base synthesis reaction is 30° C. to 50° C. and lasts for 30 minutes.

[0104] In this embodiment, the inner sidewalls of the filling holes 34 on the polydimethylsiloxane film 33 are treated to introduce active aldehyde sites, which can undergo an aldol condensation reaction with the polyvinyl alcohol in the ionic polymer gel layer 35, thereby forming a stronger adhesion at the sidewalls of the sensing site.

[0105] S623 : attaching the polydimethylsiloxane film 33 to the template 4 , and aligning the filling hole 34 with the protruding structure 41 .

[0106] S624: Filling the filling hole 34 with an ionic polymer gel layer 35 to form a sensing site.

[0107] In this step, the configured ionic polymer gel solution can be poured into the arrayed filling holes at a fixed point and in a fixed quantity by microelectronic printing technology or scraping technology, and then placed in a vacuum drying oven for evacuation, so that the ionic polymer gel solution can fully flow into the groove microstructure 41 on the protruding structure.

[0108] Then, the polydimethylsiloxane film is placed in a drying oven to fully evaporate the solvent to form an ionic polymer gel layer 35, and at the same time, the polydimethylsiloxane film with aldehyde groups after surface treatment and the polyvinyl alcohol in the ionic polymer gel layer 35 undergo an aldol condensation reaction to form a strong interface bond. Finally, the template 4 is peeled off to form the arrayed ionic medium layer.

[0109] It should be noted that the ionic polymer gel solution may include polyvinyl alcohol, ionic liquid and solvent, and the ionic gel mixed solution is obtained by mixing the polyvinyl alcohol, ionic liquid and solvent. The mass ratio of the polyvinyl alcohol to the solvent is 1:8 to 1:12, and the mass ratio of the ionic liquid to the polyvinyl alcohol is 0.5:1 to 1:1.

[0110] In this embodiment, the solvent may be distilled water, and the ionic liquid may be phosphoric acid or 1-hexyl-3-methylimidazole tricyclomethane.

[0111] S630: Laminating the arrayed ion medium layer between the first array electrode and the second array electrode to form the flexible tactile sensor array.

[0112] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A flexible tactile sensor array, characterized in that: include: A first array electrode and a second array electrode arranged opposite to each other; an arrayed ion medium layer disposed between the first array electrode and the second array electrode; The arrayed ion medium layer includes a plurality of sensing sites arranged in an array. A side of the sensing site close to the first array electrode is a planar structure, and a side of the sensing site close to the second array electrode is a protruding microstructure.

2. The flexible tactile sensor array according to claim 1, characterized in that: The arrayed ion medium layer includes a polydimethylsiloxane film with a plurality of array filling holes and a plurality of ion polymer gel layers; A plurality of the ionic polymer gel layers are respectively filled in the filling holes to form the sensing sites.

3. The flexible tactile sensor array according to claim 1, characterized in that: The protruding microstructure includes any one of a pyramid structure, a cone structure and a columnar structure.

4. A method for preparing a flexible tactile sensor array, characterized in that: Used to prepare the flexible tactile sensor array according to any one of claims 1 to 3, the preparation method comprising: forming a first array electrode and a second array electrode; forming an arrayed ion medium layer; The arrayed ion medium layer is attached between the first array electrode and the second array electrode to form the flexible tactile sensor array.

5. The preparation method according to claim 4, characterized in that: The forming of the first array electrode and the second array electrode comprises: providing a flexible substrate; Disposing a flexible electrode material on the flexible substrate to form an array electrode; Wherein, the array electrode includes the first array electrode and the second array electrode.

6. The preparation method according to claim 5, characterized in that: The flexible substrate is made of polydimethylsiloxane, and the thickness of the flexible substrate is 50-200 μm.

7. The preparation method according to claim 5, characterized in that: The flexible electrode material includes any one of silver nanofiber, liquid metal, nanosheet ink, carbon nanotube and nanowire.

8. The preparation method according to claim 5, characterized in that: The array electrodes are formed on the flexible substrate by using a laser marker, printing technology or inkjet printing technology.

9. The preparation method according to claim 4, characterized in that: The forming of the arrayed ion medium layer comprises: Providing a template having an array of protrusion structures, each of which is provided with a plurality of groove microstructures; Providing a polydimethylsiloxane film having a plurality of array-filled holes; Laminating the polydimethylsiloxane film on the template, with the filling hole aligned with the protruding structure; An ionic polymer gel layer is filled in the filling hole to form a sensing site.

10. The preparation method according to claim 9, characterized in that: The plurality of groove microstructures include any one of a pyramid structure, a cone structure and a columnar structure.

11. The preparation method according to claim 10, characterized in that: The step of filling the filling hole with an ionic polymer gel layer to form a sensing site comprises: The ionic polymer gel solution is filled into the groove microstructure through the filling holes to form a protruding microstructure.

12. The preparation method according to claim 9, characterized in that: Before providing a polydimethylsiloxane film having a plurality of array-filled holes, the method comprises: Cutting the polydimethylsiloxane isolation film with a laser to obtain the filling hole; Treating the inner sidewalls of the filling holes with plasma to form dense active silicon-oxygen groups on the inner sidewalls of the filling holes; placing the polydimethylsiloxane film treated with plasma into a prepared silane coupling agent solution for amination; The aminated polydimethylsiloxane film is immersed in a glutaraldehyde mixed solution to cause a Schiff base synthesis reaction.

13. The preparation method according to claim 12, characterized in that: The step of treating the inner sidewall of the filling hole with plasma comprises: The plasma processing power is set to 40-60W and the operation is continued for 30-60s.

14. The preparation method according to claim 12, characterized in that: The silane coupling agent solution comprises 3-aminopropyltriethoxysilane, ethanol and deionized water; wherein, The volume fraction of 3-aminopropyltriethoxysilane in the silane coupling agent solution is 15% to 30%, the volume fraction of ethanol is 30% to 50%, and the volume fraction of deionized water is 30% to 50%.

15. The preparation method according to claim 12, characterized in that: The volume fraction of the aqueous solution in the glutaraldehyde mixed solution is 2% to 10%, and the reaction temperature is 30° C. to 50° C.

16. The preparation method according to claim 11, characterized in that: The ionic polymer gel solution comprises polyvinyl alcohol, ionic liquid and solvent; wherein, The mass ratio of the polyvinyl alcohol to the solvent is 1:8 to 1:12, and the mass ratio of the ionic liquid to the polyvinyl alcohol is 0.5:1 to 1:1.

Citation Information

Cited By

  • Matrix type capacitive pressure sensing device and sensing method thereof

    CN121068061A