Detection reagent and detection method for detecting content of SPS and MPS in acid copper electroplating solution

By using specific detection reagents and ultraviolet spectrophotometry in the copper acid electroplating solution, the accuracy and detection limit of SPS and MPS content detection in the prior art are solved, and the accuracy of SPS and MPS in the copper acid electroplating solution is achieved. Quantitative analysis reduces inspection costs and equipment requirements.

CN118980675APending Publication Date: 2024-11-19UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153956.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing methods are not accurate when detecting the content of SPS and MPS in copper acid electroplating solution, and cannot distinguish the two, and the detection limit is high, which affects the electroplating implementation effect and product quality.

Method used

Using a detection reagent including a precipitant, a reducing agent, a quencher, a buffer solution and a color developer, the content of SPS and MPS in the copper acid plating solution can be measured simultaneously through the principle of ultraviolet spectrophotometry, and NaBH4 or KBH4 is used as Reducing agent, 5,5'-dithiobis(2-nitrobenzoic acid) or 4,4'-dipyridine disulfide as color developer, combines strong alkali and acid solution to adjust the pH value to improve detection accuracy.

Benefits of technology

Accurate quantitative analysis of SPS and MPS is achieved, the detection limit is reduced, the operation is simple, the equipment does not require expensive instruments, the cost is low, the repeatability is good, the detection accuracy is high, and the detection limit is 11.1μg/L.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980675A_ABST
    Figure CN118980675A_ABST
Patent Text Reader

Abstract

The invention provides a detection reagent and a detection method for detecting the content of SPS and MPS in an acid copper electroplating solution, and belongs to the technical field of electroplating solution component analysis. According to the invention, a reducing agent with higher reduction efficiency on SPS disulfide bonds and a color developing agent with higher molar absorption coefficient and wider applicable pH range are innovatively screened out, and are matched with a precipitator, a quencher and a buffer solution to form a detection reagent; by adopting the detection reagent and based on the principle of ultraviolet spectrophotometry, a detection method capable of simultaneously determining the content of SPS and MPS in the acid copper plating solution is established, and compared with other methods, equipment is simple, operation is convenient and fast, repeatability is good, and the content of MPS and SPS in the acid copper plating solution can be quantitatively analyzed at the same time; meanwhile, the detection limit is lower, the MPS detection limit is 11.1 micrograms / L, and the SPS detection limit is 11 micrograms / L.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating solution component analysis, and particularly relates to a detection reagent and a detection method for detecting the contents of SPS and MPS in an acid copper electroplating solution. Background Art

[0002] In the electronics industry, metallic copper has a wide range of application scenarios due to its outstanding performance in electrical conductivity, ductility, thermal conductivity, etc., such as integrated circuits, packaging substrates, and printed circuit boards. Electroplated copper technology is the key technology to achieve the adaptability of copper in related application scenarios. Electroplated copper technology has gone through the development process of cyanide, pyrophosphate and sulfuric acid systems. After 1985, people introduced additives into the acid copper sulfate plating solution and successfully obtained a copper coating with uniform and fine grains. Since then, a large number of additives for the acid copper sulfate plating solution system have been developed and applied in industrial production. Subsequently, in the subsequent development, it gradually replaced the environmentally unfriendly cyanide copper plating technology and the high-cost pyrophosphate copper plating technology. It is the development and application of the new additive system that has made acid copper plating the most widely used copper electroplating method in the field of electronics manufacturing.

[0003] The additives in the acid copper sulfate electroplating solution mainly refer to organic compounds. According to their role in the copper electroplating process, the additives can be divided into three categories: accelerators, inhibitors and levelers. Among them, the accelerator is the most widely studied additive among the three types of acid copper sulfate additives. In the electroplating process, it is conducive to the formation of copper crystal nuclei, plays a role in refining grains, and makes the deposited layer dense and smooth. Sodium polydisulfide propane sulfonate (SPS, CAS: 27206-35-5) and sodium 3-mercapto-1-propane sulfonate (MPS, CAS: 17636-10-1) are the most common accelerators in the acid copper sulfate electroplating system. The mechanism of action with a high acceptance rate at present is that one molecule of SPS decomposes into two molecules of MPS in the electroplating solution. The mercapto group at one end of MPS is fixed on the copper surface, and the sulfonic acid group at the other end captures the copper ions in the electroplating solution. With the assistance of chloride ions, the copper ions are accelerated to obtain electrons and reduced to metallic copper. This process improves the efficiency of copper reduction, thereby accelerating copper deposition. Studies have shown that within the potential range of copper electrodeposition, the chemical and electrochemical properties of the SPS molecule itself are relatively active, and its accelerating effect in the electroplating reaction is mainly due to the cleavage of the disulfide bonds in the SPS molecule under the action of the electric field to form MPS. However, the effects of MPS and SPS will change with concentration. When the concentration of SPS is less than 100μg / L, it will inhibit the electroplating of copper; when the concentration is higher than 100μg / L, it will promote the electroplating process of copper, but too high a concentration will cause the coating to turn white and brittle. The method currently used in industry to quantitatively analyze the content of additives in acid copper plating solutions is cyclic voltammetric stripping (CVS). The principle of this method is to quantitatively analyze the concentration of the accelerator based on the linear relationship between the amount of copper deposition and the concentration of the accelerator. However, the accuracy of this method is not high. On the one hand, it is limited by the reduction efficiency of the disulfide bonds of SPS under the action of the electric field. On the other hand, its detection results are easily affected by substances that can affect the copper deposition rate, such as Cl - In addition, this method cannot distinguish between MPS and SPS, and can only measure the concentration of the common form of the two, and the detection limit is relatively high (0.3mg / L), and it is impossible to more accurately obtain the exact concentration of MPS and SPS in the plating solution. Therefore, the above factors seriously affect the electroplating implementation effect and product quality.

[0004] In view of the above problems, some methods for quantitative analysis of MPS and SPS have been developed. Chinese patent application CN115754072A discloses a method for qualitative and quantitative determination of sodium thiopropane sulfonate brightener in acid copper electroplating solution. Polysodium disulfide propane sulfonate SPS is dissolved in sulfuric acid aqueous solution, and standard solutions of different concentrations are prepared and injected into a high performance liquid chromatography-mass spectrometer, and an ammonium acetate aqueous solution / acetonitrile is used as the mobile phase to draw a standard curve; then the acid copper electroplating solution containing sodium disulfide propane sulfonate is tested by the same method, and the content of sodium disulfide propane sulfonate in the acid copper electroplating solution is calculated according to the standard curve. However, the instruments and equipment required for this scheme are expensive, and at the same time, the acid copper solution entering the chromatographic column will corrode and consume the chromatographic column, increasing the detection cost. Chinese patent application CN 111157520A discloses a detection reagent and a detection method for detecting the content of sodium disulfide propane sulfonate in acid copper electroplating solution. The detection reagent used includes a reducing agent, a buffer solution and a color developer. The sodium polydisulfide propane sulfonate is reduced to a thiol compound by a reducing agent, and the color developer reacts with the thiol compound produced by the reduction, and the product has strong absorption at a specific wavelength. The content of sodium polydisulfide propane sulfonate in the acid copper electroplating solution can be calculated based on the relationship between the absorption intensity and the standard curve. However, the molar absorption coefficient of the color developer 5,5'-dithiobis(2-nitrobenzoic acid) used in this method is not high, resulting in a detection limit of up to 2μmol / L (0.7mg / L) for this detection method. At the same time, the reducing agent mentioned in the patent itself has a thiol group and has not been completely removed, which will affect the accuracy of the detection result.

[0005] Therefore, it is particularly important to develop a method that is more suitable for actual use in enterprise factories, easy to operate, simple in process and can accurately determine the content of SPS and MPS in the plating solution. Summary of the invention

[0006] In view of the problems existing in the background technology, the purpose of the present invention is to provide a detection reagent and a detection method for detecting the content of SPS and MPS in the acid copper electroplating solution. The present invention innovatively screens out a reducing agent with higher efficiency in reducing the disulfide bonds of SPS, and a color developer with higher molar absorption coefficient and wider applicable pH range, and then matches a precipitant quencher and a buffer solution to form a detection reagent; using the detection reagent, based on the principle of ultraviolet spectrophotometry, a detection method that can simultaneously determine the content of SPS and MPS in the acid copper electroplating solution is established, which is simpler than other methods, convenient to operate, has a lower detection limit, good repeatability, and can simultaneously quantitatively analyze the content of MPS and SPS in the acid copper plating solution.

[0007] To achieve the above object, the technical solution of the present invention is as follows:

[0008] A detection reagent for detecting the content of SPS and MPS in an acid copper electroplating solution, comprising a precipitant, a reducing agent, a quencher, a buffer solution and a developer solution; the precipitant is a strong base for adjusting the pH value of the plating solution and precipitating metal interfering ions; the reducing agent is a NaBH4 solution or a KBH4 solution for reducing SPS in the acid copper electroplating solution; the quencher is a strong acid solution for removing excess reducing agent; the developer solution is a 5,5'-dithiobis(2-nitrobenzoic acid) (DTNB) solution or a 4,4'-dipyridyl disulfide (DTDP) solution; and the buffer solution is used to create a suitable color development environment for the developer.

[0009] Furthermore, the strong base is NaOH or KOH.

[0010] Furthermore, the NaBH4 solution or KBH4 solution is prepared by dissolving solid NaBH4 or KBH4 in an alkaline solution of a certain concentration, the alkaline solution is a NaOH or KOH solution with a concentration of 0.1 to 2 mol / L; the concentration of the reducing agent is 1 to 6 mol / L.

[0011] Furthermore, the quencher is a hydrochloric acid solution, a sulfuric acid solution or a nitric acid solution, and the H + The concentration is 1~8mol / L.

[0012] Furthermore, if the developer solution is a 5,5'-dithiobis(2-nitrobenzoic acid) solution, the buffer solution should be a buffer solution with a pH value of 7 to 8; if the developer solution is a 4,4'-bipyridyl disulfide solution, the buffer solution should be a buffer solution with a pH value of 4.5 to 6;

[0013] The 5,5'-dithiobis(2-nitrobenzoic acid) solution is a solution obtained by dissolving solid 5,5'-dithiobis(2-nitrobenzoic acid) in a buffer solution with a pH value of 7 to 8. If the pH is greater than 8.2, 5,5'-dithiobis(2-nitrobenzoic acid) will become ineffective in a short time and affect the test. If the pH is too low, the solid is difficult to dissolve. The 4,4'-bipyridine disulfide solution is a solution obtained by dissolving solid 4,4'-bipyridine disulfide in a dilute hydrochloric acid solution.

[0014] Furthermore, the buffer with a pH value of 4.5 to 6 is an acetate buffer, a citrate-phosphate buffer or a phosphate buffer; and the buffer with a pH value of 7 to 8 is a phosphate buffer.

[0015] Furthermore, the concentration of the developer is determined according to the concentration of the liquid to be tested. Generally, the molar amount of the developer is at least 100 times the molar amount of the substance to be tested, and the concentration is preferably greater than 1 μmol / L.

[0016] Furthermore, the acid copper plating solution includes H2SO4, Cl -, CuSO4·5H2O, an inhibitor and a leveler, wherein the inhibitor is preferably PEG-8000, and the leveler is preferably Jiana Green B; wherein the concentration of H2SO4 is less than 300g / L, Cl - The concentration of is less than 150g / L, the concentration of CuSO4·5H2O is less than 150g / L, the concentration of PEG-8000 is less than 3000mg / L, and the concentration of Janus Green B is less than 50mg / L.

[0017] A method for detecting the content of SPS and MPS in an acid copper electroplating solution comprises the following steps:

[0018] Step 1. Draw the MPS standard curve. The specific process is as follows:

[0019] Step 1.1. Prepare MPS standard solution, the specific process is: dissolve solid MPS in deionized water to obtain a MPS standard solution of a certain concentration;

[0020] Step 1.2. Pipette different volumes of MPS standard solution into multiple colorimetric tubes, add a certain amount of buffer solution, shake well, add a certain amount of color developer solution, add water to the same scale line, and then obtain MPS solutions of different concentrations. The type of buffer solution is determined according to the type of color developer added.

[0021] Step 1.3. Determine the absorbance of MPS solutions of different concentrations: wait for the MPS solutions of different concentrations to react for a period of time, then add the first reference solution to the ultraviolet spectrophotometer to clear the absorbance, and then use the ultraviolet spectrophotometer to measure the absorbance of the MPS solutions of different concentrations at the wavelength corresponding to the color developer; wherein the first reference solution is the MPS solution with a volume of 0 in the MPS standard solution in step 1.2;

[0022] Step 1.4. Determine the MPS standard curve equation: In a coordinate system where the horizontal axis is concentration and the vertical axis is absorbance, fit the absorbance of MPS solutions of different concentrations to obtain the standard linear curve equation, which is A=ac+b, where the unit of A is abs, the unit of c is mol / L, and a and b are both constants;

[0023] Step 2. Prepare the test solution. The specific process is as follows:

[0024] Step 2.1. Obtaining an acid copper electroplating solution to be tested containing both MPS and SPS;

[0025] Step 2.2. Add a precipitant to the acid copper electroplating solution to be tested and adjust the pH of the acid copper electroplating solution to a strong alkaline state to remove the metal interfering ions (Cu 2+ ,Fe 2+ ,Fe 3+ ,Ni 2+,Pb 2+ etc.) to prevent affecting subsequent detection; then centrifuge at a certain speed for a certain time to separate the solid and liquid, and then take the supernatant as the test liquid;

[0026] Step 3. Determine the concentration of the thiol compound in the test solution in step 2. The specific process is as follows:

[0027] Step 3.1. Take two equal volumes of the test solution obtained in step 1.1, and place the two supernatants in two test tubes respectively, add the reducing agent solution to one test tube, and add the same volume of reducing agent solution to the other test tube, the alkaline solution is the same as the alkaline solution in the reducing agent; the reducing agent solution only does not contain the reducing agent, and the other components and contents are the same as the reducing agent solution;

[0028] Step 3.2. After the reduction reaction is fully reacted, the quencher is added. After the reaction is complete, the buffer solution and the color developer solution are added in sequence. Finally, the volume is adjusted to the required volume with pure water, and the mixture is fully mixed by ultrasound. The pH of the buffer solution is different depending on the color developer used.

[0029] Step 3.3. Add a second reference solution to the UV spectrophotometer to clear the absorbance to zero, and then use the UV spectrophotometer to measure the absorbance of the two test solutions obtained in step 3.2 at the wavelength corresponding to the color developer; wherein the composition of the second reference solution is the same as that of the test solution in step 2.2, except that SPS and MPS are not included;

[0030] Step 3.4. Substitute the absorbance into the MPS standard curve equation obtained in step 2 to obtain the MPS content existing in the acid copper electroplating solution and the total MPS content; wherein, the MPS content existing in the acid copper electroplating solution is measured in the test tube without adding the reducing agent, and the MPS content in the acid copper electroplating solution is measured in the test tube with adding the reducing agent;

[0031] Step 4. Calculate the SPS content in the plating solution. The specific process is:

[0032] According to the relationship between the dilution multiple of the acid copper plating solution and the reduction of SPS, and in combination with the MPS and total MPS content obtained in step 3, the content of SPS in the acid copper plating solution is calculated.

[0033] Furthermore, in step 2.2, the centrifugal speed is not less than 3000 r / min, and the centrifugal time is not less than 20 min.

[0034] The mechanism of the present invention is as follows: the color developer DTNB or DTDP used in the present invention only reacts with MPS but does not react with SPS. If there is only MPS in the plating solution, it is not necessary to add a reducing agent for quantitative analysis of MPS at this time, and the color developer can be directly added for determination; when SPS and MPS coexist in the plating solution, if SPS is to be quantitatively analyzed, it is necessary to first add a reducing agent to reduce SPS to MPS, and then use a color developer to test the total content of MPS. At this time, the total content includes the MPS that initially exists and the MPS content generated by the reduction of SPS. The initial MPS content measured without adding the reducing agent is subtracted from the total MPS content to obtain the MPS content generated by the reduction of SPS, and then the SPS content can be obtained according to the relationship that one SPS is reduced to generate two MPS contents, thereby achieving quantitative analysis of SPS and MPS respectively.

[0035] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0036] 1. The reducing agent used in the present invention is NaBH4 or KBH4. Based on its reducing property to reduce disulfide bonds, when it is mixed with a solution containing SPS, SPS can be completely reduced to MPS. At the same time, excess NaBH4 or KBH4 can be completely quenched by the acid solution without affecting subsequent experiments.

[0037] 2. Both color developers used in the present invention can be used to detect thiol compounds generated by the reduction of SPS in the acid copper plating solution. Among them, the pH range required for the maximum absorption absorbance of DTDP is 3-6, and the pH range required for the maximum absorption absorbance of DTNB is 7-8. Of the two, DTDP requires a wider pH range for the maximum absorption absorbance and is acidic, so it is more suitable for the acidic system of the acid copper plating solution. In actual tests, it was found that its sensitivity for detecting thiol compounds in the acid copper plating solution was nearly 50% higher than that of the same type of color developer DTNB.

[0038] 3. The detection method of the present invention can restore SPS without complicated operations, and can more accurately determine the contents of SPS and MPS in the plating solution, and has low detection cost, does not require expensive equipment, is quick to operate, has high detection accuracy, good repeatability, and a low detection limit (11.1 μg / L for MPS and 11 μg / L for SPS). BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a graph of the MPS standard curve obtained in Example 1 of the present invention.

[0040] Figure 2 This is a data diagram of the quantitative analysis results of Example 1 of the present invention.

[0041] Figure 3This is a graph of the MPS standard curve obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0042] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the implementation modes and the accompanying drawings.

[0043] Example 1

[0044] The specific composition of the acid copper electroplating solution to be tested containing MPS and SPS in this embodiment is: 200g / L H2SO4, 60mg / L Cl - (from HCl), 75 g / L CuSO 4· 5H2O, 300mg / L PEG-8000, 5mg / L JGB; MPS and SPS with the same mass concentration were also included, and four different concentrations were selected to prepare four acid copper electroplating solutions to be tested, with concentrations of 0mg / L, 2mg / L (C mps =11.22μmol / L, C sps =5.64μmol / L), 4mg / L(C mps =22.45μmol / L, C sp s =11.29μmol / L), 6mg / L(C mps =33.67 μmol / L, C sps =16.93 μmol / L).

[0045] A method for detecting the content of SPS and MPS in an acid copper electroplating solution comprises the following steps:

[0046] Step 1. Draw the MPS standard curve. The specific process is as follows:

[0047] Step 1.1. Weigh 0.0556 g of solid MPS (wherein the effective mass of MPS is 0.0500 g), dissolve the solid MPS in deionized water, transfer to a 1 L volumetric flask and dilute to obtain a MPS standard solution with a concentration of 280.57 μmol / L (50 mg / L);

[0048] Step 1.2. Pipette 0 μL, 25 μL, 50 μL, 75 μL, 100 μL, 125 μL, 150 μL, 200 μL, 300 μL, 400 μL, 500 μL, 600 μL, 700 μL, 800 μL, 1000 μL, and 1250 μL of MPS standard solution into 16 25 mL colorimetric tubes, add 20 mL of NaH2HPO4-EDTA·2Na buffer solution with a pH of 4.5, shake well, add 1 mL of DTDP solution, and finally add pure water to make up to volume, and stir vigorously to obtain MPS solutions of different concentrations;

[0049] Step 1.3. Determine the absorbance of MPS solutions of different concentrations: After the MPS solutions of different concentrations react for 20 minutes, add the first reference solution to clear the absorbance in the ultraviolet spectrophotometer, and then use the ultraviolet spectrophotometer to determine the absorbance of the solutions in the remaining groups of colorimetric tubes at 324 nm; wherein the reference solution is the MPS solution with a volume of 0 of the MPS standard solution in step 1.2;

[0050] Step 1.4. Determine the MPS standard curve equation: With the MPS concentration (mol / L) as the abscissa and the absorbance as the ordinate, fit the absorbance of MPS solutions of different concentrations, draw the absorbance-concentration standard curve, and establish the MPS standard curve equation, such as Figure 1 As shown, that is: A = 26484.34c + 2.6 × 10 -4 , where R 2 =0.9992, the unit of c is mol / L;

[0051] Step 2. Prepare the test solution. The specific process is as follows:

[0052] Step 2.1. Obtain three portions of the acid copper electroplating solution to be tested with different concentrations and containing both MPS and SPS, each with a volume of 20 mL;

[0053] Step 2.2. Add 4g of solid NaOH precipitant to the acid copper electroplating solution to be tested and stir vigorously to remove the metal interfering ions (Cu 2+ ,Fe 2+ ,Fe 3+ ,Ni 2+ ,Pb 2+ After cooling to room temperature, centrifuge at 6000r / min for 20min, and take the supernatant as the test solution;

[0054] Step 3. Determine the concentration of the thiol compound in the test solution of step 2, the specific process is:

[0055] Step 3.1. Prepare a NaBH4 solution (BH) with a concentration of 5.3 mol / L, wherein the NaBH4 solution is obtained by dissolving solid NaBH4 in a NaOH solution with a concentration of 1 mol / L;

[0056] Step 3.2. For each sample solution, 1 mL of the sample solution obtained in step 2.2 was respectively transferred into two 25 mL colorimetric tubes, 2 mL of 5.5 mol / L BH solution was added to one colorimetric tube, and 2 mL of 1 mol / L NaOH solution was added to the other colorimetric tube, and then the two colorimetric tubes were kept in a water bath (75°C) for 20 min;

[0057] Step 3.3. After the reduction reaction is fully reacted, add 2 mL of 5 mol / L HCl solution. During the process, shake the colorimetric tube continuously until no visible bubbles are generated in the test solution (about 3 minutes). After the reaction is complete, add 20 mL of pH = 4.5 NaH2HPO4-EDTA·2Na buffer, then add 1 mL of DTDP solution, and finally add pure water to make up the volume and stir vigorously;

[0058] Step 3.4. After the color development reaction for 20 minutes, add a second reference solution to the UV spectrophotometer to clear the absorbance, and then use the UV spectrophotometer to measure the absorbance of all test solutions at 324nm; the composition of the second reference solution is the same as that of the test solution in step 2.2, except that SPS and MPS are not included;

[0059] Step 3.5. Substitute the absorbance into the MPS standard curve equation obtained in step 1 to obtain the MPS content and the total MPS content in the dilution solution in step 3.2; wherein, the MPS content in the acid copper electroplating solution is measured in the test tube without adding the reducing agent, and the total MPS content in the acid copper electroplating solution is measured in the test tube with adding the reducing agent;

[0060] Step 4. Calculate the SPS content in the plating solution. The specific process is:

[0061] The MPS originally existing in the dilution solution and the total MPS content are obtained. The difference between the two can be used to obtain the MPS content generated by the reduction of SPS. According to the dilution multiple, the MPS and SPS contents in the acid copper plating solution can be obtained.

[0062] The above operation was repeated 5 times for each concentration of the acid copper electroplating solution containing MPS and SPS. The obtained MPS and SPS content data are shown in Figure 2 As shown in the figure, m x,mps is the detection content of MPS in the acid copper plating solution, in mg / L; is the average detected content of MPS in the acid copper plating solution, in mg / L; m x,sps is the detection content of SPS in the acid copper plating solution, in mg / L; is the average detected content of SPS in the acid copper plating solution, in mg / L; m sps and m mps The content of SPS and MPS in the prepared acid copper plating solution is in mg / L; δ mps is the relative error of MPS detected by this method, δ sps Detect the relative error of SPS for this method;

[0063] Depend on Figure 1 The standard curve equation and Figure 2It can be seen that the relative errors of the detection of MPS and SPS in the acid copper solution provided by the present invention are -9.66% to 8.25% and -9.09% to 7.64%, respectively. The minimum detection limit of MPS in the detection solution is 11.1 μg / L, and the minimum detection limit of SPS is 11 μg / L.

[0064] Example 2

[0065] A method for detecting the content of SPS and MPS in an acid copper electroplating solution comprises the following steps:

[0066] Step 1. Draw the MPS standard curve. The specific process is as follows:

[0067] Step 1.1. Weigh 0.0556 g of solid MPS (wherein the effective mass of MPS is 0.0500 g), dissolve the solid MPS in deionized water, transfer to a 1 L volumetric flask and dilute to obtain a MPS standard solution with a concentration of 280.57 μmol / L (50 mg / L);

[0068] Step 1.2. Pipette 0 μL, 25 μL, 50 μL, 75 μL, 100 μL, 125 μL, 150 μL, 200 μL, 300 μL, 400 μL, 500 μL, 600 μL, 700 μL, 800 μL, 1000 μL, and 1250 μL of MPS standard solution into 16 25 mL colorimetric tubes, add 20 mL of NaH2PO4-Na2HPO4 buffer solution with a pH of 7.8, shake well, add 1 mL of DTNB solution, and finally add pure water to make up to volume, and stir vigorously to obtain MPS solutions of different concentrations;

[0069] Step 1.3. Determine the absorbance of MPS solutions of different concentrations: After the MPS solutions of different concentrations react for 20 minutes, add the first reference solution to clear the absorbance in the ultraviolet spectrophotometer, and then use the ultraviolet spectrophotometer to determine the absorbance of the solutions in the remaining groups of colorimetric tubes at 412 nm; wherein the reference solution is the MPS solution with a volume of 0 of the MPS standard solution in step 1.2;

[0070] Step 1.4. Determine the MPS standard curve equation: With the MPS concentration (μg / L) as the abscissa and the absorbance as the ordinate, fit the absorbance of MPS solutions of different concentrations, draw the absorbance-concentration standard curve, and establish the MPS standard curve equation, such as Figure 3 As shown, that is: A = 8.7 × 10 -5 c, where R 2 =0.9992, the unit of c is μg / L;

[0071] Step 2. Prepare the test solution. The specific process is as follows:

[0072] Step 2.1. Obtain three portions of the acid copper electroplating solution to be tested with different concentrations and containing both MPS and SPS, each with a volume of 20 mL;

[0073] Step 2.2. Add 4g of solid NaOH precipitant to the acid copper electroplating solution to be tested and stir vigorously to adjust the pH of the solution to remove interfering metal ions (Cu 2+ ,Fe 2+ ,Fe 3+ ,Ni 2+ ,Pb 2+ etc.) to prevent residual metal ions from affecting subsequent detection; after cooling to room temperature, centrifuge at 6000r / min for 20min, and take the supernatant as the test solution;

[0074] Step 3. Determine the concentration of the thiol compound in the test solution of step 2, the specific process is:

[0075] Step 3.1. Prepare a KBH4 solution with a concentration of 5.3 mol / L, wherein the KBH4 solution is obtained by dissolving solid KBH4 in a NaOH solution with a concentration of 1 mol / L;

[0076] Step 3.2. For each sample solution, 1 mL of the sample solution obtained in step 2.2 was respectively transferred into two 25 mL colorimetric tubes, 2 mL of 5.5 mol / L BH solution was added to one colorimetric tube, and 2 mL of 1 mol / L NaOH solution was added to the other colorimetric tube, and then the two colorimetric tubes were kept in a water bath (75°C) for 20 min;

[0077] Step 3.3. After the reduction reaction is fully reacted, add 2 mL of 5 mol / L HCl solution, and shake the colorimetric tube continuously during the process until no visible bubbles are generated in the test solution (approximately 3 minutes). After the reaction is complete, add 20 mL of pH = 7.8 NaH2HPO4-Na2HPO4 buffer (including 1 mmol / L EDTA·2Na), and then add 1 mL of DTDP solution, wherein the DTDP solution is obtained by dissolving solid DTDP in 0.2 mol / L dilute hydrochloric acid solution, and finally add pure water to make up the volume and stir vigorously;

[0078] Step 3.4. After the color development reaction for 20 minutes, add a second reference solution to the UV spectrophotometer to clear the absorbance, and then use the UV spectrophotometer to measure the absorbance of all test solutions at 412 nm; the composition of the second reference solution is the same as that of the test solution in step 2.2, except that SPS and MPS are not included;

[0079] Step 3.5. Substitute the absorbance into the MPS standard curve equation obtained in step 1 to obtain the MPS content and the total MPS content in the dilution solution in step 3.2; wherein, the MPS content in the acid copper electroplating solution is measured in the test tube without adding the reducing agent, and the total MPS content in the acid copper electroplating solution is measured in the test tube with adding the reducing agent;

[0080] Step 4. Calculate the SPS content in the plating solution. The specific process is:

[0081] The original MPS and total MPS content in the dilution solution were obtained, and the difference between the two was the MPS content produced by SPS reduction. According to the dilution multiple, the MPS and SPS contents in the acid copper plating solution were obtained.

[0082] The above description is only a specific implementation mode of the present invention. Any feature disclosed in this specification, unless otherwise stated, can be replaced by other alternative features that are equivalent or have similar purposes; all the disclosed features, or all the steps in the methods or processes, except for mutually exclusive features and / or steps, can be combined in any way.

Claims

1. A detection reagent for detecting the content of SPS and MPS in an acid copper electroplating solution, characterized in that: The invention comprises a precipitant, a reducing agent, a quencher, a buffer solution and a developer solution; the precipitant is a strong base for adjusting the pH value of the plating solution and precipitating metal interfering ions; the reducing agent is a NaBH4 solution or a KBH4 solution for reducing SPS in the acid copper electroplating solution; the quencher is a strong acid solution for removing excess reducing agent; the developer solution is a 5,5'-dithiobis(2-nitrobenzoic acid) solution or a 4,4'-bipyridine disulfide solution; and the buffer solution is used to create a suitable color development environment for the developer.

2. The detection reagent according to claim 1, characterized in that The strong base is NaOH or KOH.

3. The detection reagent according to claim 1, characterized in that The NaBH4 solution or KBH4 solution is prepared by dissolving solid NaBH4 or KBH4 in an alkaline solution of a certain concentration, wherein the alkaline solution is a NaOH or KOH solution with a concentration of 0.1 to 2 mol / L; and the concentration of the reducing agent is 1 to 6 mol / L.

4. The detection reagent according to claim 1, characterized in that The quencher is a hydrochloric acid solution, a sulfuric acid solution or a nitric acid solution, and H + The concentration is 1~8mol / L.

5. The detection reagent according to claim 1, characterized in that If the color developer solution is 5,5'-dithiobis(2-nitrobenzoic acid) solution, the buffer solution should be a buffer solution with a pH value of 7 to 8; if the color developer solution is 4,4'-bipyridyl disulfide solution, the buffer solution should be a buffer solution with a pH value of 4.5 to 6; The 5,5'-disulfide bis(2-nitrobenzoic acid) solution is a solution obtained by dissolving solid 5,5'-disulfide bis(2-nitrobenzoic acid) in a buffer solution with a pH value of 7 to 8, and the 4,4'-bipyridyl disulfide solution is a solution obtained by dissolving solid 4,4'-bipyridyl disulfide in a dilute hydrochloric acid solution.

6. The detection reagent according to claim 5, characterized in that The buffer with a pH value of 4.5 to 6 is acetate buffer, citrate-phosphate buffer or phosphate buffer; the buffer with a pH value of 7 to 8 is phosphate buffer.

7. The detection reagent according to claim 1, characterized in that The concentration of the developer is determined according to the concentration of the solution to be tested.

8. The detection reagent according to claim 1, characterized in that The acid copper plating solution includes H2SO4, Cl - , CuSO4·5H2O, inhibitor and leveler; wherein the concentration of H2SO4 is less than 300g / L, Cl - The concentration of is less than 150g / L, the concentration of CuSO4·5H2O is less than 150g / L, the concentration of inhibitor is less than 3000mg / L, and the concentration of leveling agent is less than 50mg / L.

9. A method for detecting the content of SPS and MPS in an acid copper electroplating solution, characterized in that: The following steps are involved: Step 1. Draw the MPS standard curve. The specific process is as follows: Step 1.

1. Prepare MPS standard solution, the specific process is: dissolve solid MPS in deionized water to obtain a MPS standard solution of a certain concentration; Step 1.

2. Pipette different volumes of MPS standard solution into multiple colorimetric tubes, add a certain amount of buffer solution, shake well, add a certain amount of color developer solution, add water to the same scale line, and then obtain MPS solutions of different concentrations. The type of buffer solution is determined according to the type of color developer added. Step 1.

3. Determine the absorbance of MPS solutions of different concentrations: wait for the MPS solutions of different concentrations to react for a period of time, then add the first reference solution to the ultraviolet spectrophotometer to clear the absorbance, and then use the ultraviolet spectrophotometer to measure the absorbance of the MPS solutions of different concentrations at the wavelength corresponding to the color developer; wherein the first reference solution is the MPS solution with a volume of 0 in the MPS standard solution in step 1.2; Step 1.

4. Determine the MPS standard curve equation: In a coordinate system where the horizontal axis is concentration and the vertical axis is absorbance, fit the absorbance of MPS solutions of different concentrations to obtain the standard linear curve equation, which is A=ac+b, where the unit of A is abs, the unit of c is mol / L, and a and b are both constants; Step 2. Prepare the test solution. The specific process is as follows: Step 2.

1. Obtaining an acid copper electroplating solution to be tested containing both MPS and SPS; Step 2.

2. Add a precipitant to the acid copper electroplating solution to be tested, adjust the pH of the acid copper electroplating solution to a strong alkaline state, so as to remove metal ions in the acid copper electroplating solution and prevent residual metal ions from affecting subsequent detection; then centrifuge at a certain speed for a certain time to separate the solid and liquid layers, and then take the supernatant as the test solution; Step 3. Determine the concentration of the thiol compound in the test solution in step 2. The specific process is as follows: Step 3.

1. Take two equal volumes of the test solution obtained in step 1.1, and place the two supernatants in two test tubes respectively, add the reducing agent solution to one test tube, and add the same volume of reducing agent solution to the other test tube, the alkaline solution is the same as the alkaline solution in the reducing agent; the reducing agent solution only does not contain the reducing agent, and the other components and contents are the same as the reducing agent solution; Step 3.

2. After the reduction reaction is fully reacted, the quencher is added. After the reaction is complete, the buffer solution and the color developer solution are added in sequence. Finally, the volume is adjusted to the required volume with pure water, and the mixture is fully mixed by ultrasound. The pH of the buffer solution is different depending on the color developer solution used. Step 3.

3. Add a second reference solution to the UV spectrophotometer to clear the absorbance to zero, and then use the UV spectrophotometer to measure the absorbance of the two test solutions obtained in step 3.2 at the wavelength corresponding to the color developer; wherein the composition of the second reference solution is the same as that of the test solution in step 2.2, except that SPS and MPS are not included; Step 3.

4. Substitute the absorbance into the MPS standard curve equation obtained in step 2 to obtain the MPS content existing in the acid copper electroplating solution and the total MPS content; wherein, the MPS content existing in the acid copper electroplating solution is measured in the test tube without adding the reducing agent, and the MPS content in the acid copper electroplating solution is measured in the test tube with adding the reducing agent; Step 4. Calculate the SPS content in the plating solution. The specific process is: According to the relationship between the dilution multiple of the acid copper plating solution and the reduction of SPS, and in combination with the MPS and total MPS content obtained in step 3, the content of SPS in the acid copper plating solution is calculated.

10. The detection method according to claim 9, characterized in that: In step 2.2, the centrifugal speed is not less than 3000 r / min, and the centrifugal time is not less than 20 min.