High-specific-energy lithium manganese iron phosphate positive electrode material and preparation method thereof

By doping rare earth element dysprosium into LiMnFePO4 positive electrode material and using biomass carbon source and polystyrene microsphere powder, combined with sintering and electrospinning technology, the problems of material conductivity and cycle life are solved, and high specific energy density and Improved stability performance.

CN118983410AActive Publication Date: 2024-11-19HUNAN SMART VALLEY NEW ENERGY TECHNOLOGY RESEARCH INSTITUTE CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411057104.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing LiMnFePO4 positive electrode materials have low electronic conductivity and low ion mobility, resulting in low actual discharge capacity and poor cycle life, making it difficult to meet the needs of high-specific energy lithium-ion batteries.

Method used

By doping rare earth element dysprosium, using biomass carbon source coating and polystyrene microsphere powder, combined with sintering, gel method and electrospinning technology, a high specific energy lithium manganese iron phosphate positive electrode material is prepared to improve its crystallization degree and pressure Real density.

Benefits of technology

The volume energy density and electrochemical properties of the material are significantly improved, with the first discharge specific capacity as high as 164.1mAh·g-1, and the capacity retention rate after 30 cycles is 98.8%, and the conductivity and cycle stability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983410A_ABST
    Figure CN118983410A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and particularly relates to a high-specific-energy lithium manganese iron phosphate positive electrode material and a preparation method thereof. The high-specific-energy lithium manganese iron phosphate positive electrode material is finally obtained by doping rare earth element dysprosium, preferably performing biomass carbon source coating and polystyrene microsphere powder treatment and combining with application of technologies such as sintering, gel method treatment and electrospinning. The problems of low electronic conductivity, low ion mobility, low actual discharge capacity of the battery, short cycle life and the like of the traditional lithium manganese iron phosphate positive electrode material are solved, and the lithium manganese iron phosphate positive electrode material has the advantages of high crystallization degree, high compaction density, high volume energy density, excellent performance and wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a high-energy lithium manganese iron phosphate positive electrode material and a preparation method thereof. Background Art

[0002] The shortage of energy supply, the rise in oil and gas prices, and a series of economic and environmental problems caused by energy issues have made people pay more and more attention to the development and use of clean energy. The storage of clean energy is also an issue worthy of attention. Converting these clean energies into electrical energy is undoubtedly the most feasible method. Lithium-ion batteries have become the first choice for energy storage due to their high energy density, high safety performance, and good environmental protection.

[0003] With the rapid development of lithium-ion batteries in the field of new energy, the current commercial lithium-ion batteries are difficult to meet people's needs for high-energy-density batteries. The development of lithium-ion battery materials with high energy-density and new high-energy-density batteries has become a research focus. Olivine-type LiMnFePO4 cathode materials have high operating voltage and theoretical specific capacity, and their low production cost and excellent safety performance are expected to be used in the high-energy-density lithium-ion secondary battery industry. However, the LiMnFePO4 cathode material has low electronic conductivity and low ion mobility, and the actual discharge capacity of the battery is low and the cycle life is poor, and the comprehensive electrochemical performance needs to be improved urgently. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a high specific energy lithium iron manganese phosphate positive electrode material and a preparation method thereof. By doping with rare earth element dysprosium, preferably coating with biomass carbon source, treating with polystyrene microsphere powder, combining sintering, gel treatment, electrospinning and other technologies, a high specific energy lithium iron manganese phosphate positive electrode material is finally obtained, which has a high degree of crystallinity and compaction density, a high volume energy density and a small degree of conductivity.

[0005] A high specific energy lithium iron manganese phosphate positive electrode material, the chemical general formula of the high specific energy lithium iron manganese phosphate positive electrode material is LiMn x Fe 1-x PO4@Dy / C / PS, x ranges from 0.6 to 0.8. Furthermore, x is 0.7. The general chemical formula of the high specific energy lithium manganese iron phosphate cathode material is LiMn 0.7 Fe 0.3 PO4@Dy / C / PS;

[0006] Preferably, in the chemical formula, Dy / C / PS represents the coating / dopant of the positive electrode material, Dy represents the rare earth element dysprosium, with an atomic number of 66 and a relative atomic mass of 162.5, C represents a carbon source, specifically polyvinyl alcohol or sodium caseinate, and PS represents polystyrene microspheres.

[0007] The method for preparing the high specific energy lithium manganese iron phosphate positive electrode material specifically comprises the following steps:

[0008] S1. Prepare the raw materials required for preparing high specific energy lithium manganese iron phosphate positive electrode material;

[0009] S2. Weigh the corresponding mass fractions of manganese source, iron source, lithium source and phosphate source according to the atomic ratio, mix and obtain a mixture 1, weigh 3%-5% of the mass of the mixture 1, mix the dysprosium sulfate with the mixture 1 and disperse it evenly, sinter at high temperature, cool naturally to room temperature, and crush to obtain a powder 1 with a particle size of 6-8μm;

[0010] S3. Powder 1, sodium caseinate and polyvinyl alcohol obtained in step S2 are weighed in a mass ratio of 1:0.06-0.1:0.08-0.12, and mixture 2 is obtained after mixing. Deionized water in an amount of 15-30 times the mass of mixture 2 is added, and then stirred at 90-100° C. for 20-30 min to obtain a gel-like substance. The gel-like substance is heated to 250-300° C. in a nitrogen atmosphere for 2-3 h, and then ground and calcined at high temperature to obtain powder 2;

[0011] S4. Preparation of polystyrene microsphere powder;

[0012] S5. Weigh the powder 2 obtained in step S3, the polystyrene microsphere powder obtained in step S4 and N,N-dimethylformamide according to a mass ratio of 1:0.1-0.2:8-15, mix them evenly to obtain a mixture 3, place the mixture 3 in a water bath, set the temperature to 50-60°C, and continue stirring for 4-5h to obtain a spinning solution;

[0013] S6. The spinning solution obtained in step S5 is made into precursor fibers using electrospinning technology, and after pre-oxidation and heat treatment in sequence, a high-energy lithium iron manganese phosphate positive electrode material is obtained.

[0014] Preferably, the raw materials in step S1 include the following substances: manganese source, iron source, lithium source, phosphate source, dysprosium sulfate, polyvinyl alcohol, sodium caseinate, polyvinyl pyrrolidone, styrene, azobisisobutyramidine hydrochloride, ethanol, N,N-dimethylformamide, and deionized water;

[0015] Preferably, the manganese source is manganese phosphate or manganese dioxide, the iron source is ferric orthophosphate, the lithium source is lithium carbonate, the phosphoric acid source is provided by manganese phosphate and ferric orthophosphate, and the insufficient part is supplemented by phosphoric acid;

[0016] Preferably, the high temperature sintering in step S2 is carried out in a nitrogen atmosphere, and the sintering temperature is 500-550° C.;

[0017] Preferably, the high temperature calcination in step S3 is carried out at 500-600° C. and continuously treated for 4-5 hours under a nitrogen atmosphere;

[0018] Preferably, in step S4, the following steps are specifically included:

[0019] S4.1. Weigh polyvinyl pyrrolidone, deionized water, and styrene in a mass-to-volume ratio of 0.1:120-150:6-8, stir the polyvinyl pyrrolidone and deionized water in a three-necked flask, add styrene after nitrogen flow for 45-60 minutes, and continue stirring at a speed of 100-120 rpm for 15-20 minutes to obtain liquid 1;

[0020] S4.2. Weigh liquid 1, azobisisobutyramidine hydrochloride and deionized water in a mass-to-volume ratio of 10:0.1-0.15:20-30, mix liquid 1, azobisisobutyramidine hydrochloride and deionized water under a nitrogen atmosphere, and continue the reaction at 75-85°C for 30-36 hours at a rotation speed of 80-120 rpm. Then, filter, wash with ethanol and dry in an oven to obtain polystyrene microsphere powder.

[0021] Preferably, in step S6, the following steps are specifically included:

[0022] S6.1, injecting the spinning solution obtained in step S5 into a plastic syringe equipped with a 20G stainless steel needle, and then fixing the syringe on a micro-injection pump, connecting one end of the needle to the positive electrode of a high-voltage electrostatic generator, and connecting a collecting device to the negative electrode of the high-voltage electrostatic generator, and performing an electrospinning operation to obtain a precursor fiber;

[0023] S6.2. Place the precursor fiber in step S6.1 at room temperature for 12-20 hours, then transfer it to a tubular sintering furnace, pre-oxidize it in air at 180-200°C for 4-5 hours, and then keep it warm at 680-720°C in an argon-hydrogen mixed atmosphere for 2-3 hours to obtain a high specific energy lithium manganese iron phosphate positive electrode material.

[0024] The beneficial effects achieved by the present invention are as follows:

[0025] The present invention is based on the concept that increasing the compaction density of lithium iron manganese phosphate positive electrode materials can effectively improve their volume energy density, and the lithium iron manganese phosphate positive electrode materials are modified multiple times, specifically as follows: doping with rare earth element dysprosium, coating with biomass carbon source, and treating with polystyrene microsphere powder, thereby improving the compaction density of the lithium iron manganese phosphate positive electrode material without reducing the electrochemical performance, and preparing a high specific energy lithium iron manganese phosphate positive electrode material.

[0026] The biomass carbon sources used in the present invention are specifically polyvinyl alcohol and sodium caseinate, which can promote the transfer of charges and improve the electrical conductivity of the material. The specific film-like coating layer formed by the polystyrene microsphere powder can reduce the specific surface area of ​​the material while ensuring that the material has a high electrical conductivity. When used as a template, it can also inhibit particle agglomeration and reduce particle size, thereby accelerating the lithium ion conduction rate and improving the diffusion coefficient of lithium ions. Finally, the electrospinning technology treatment is beneficial to the conductivity of the electrode while further improving the compaction density and can improve the yield.

[0027] The high specific energy lithium manganese iron phosphate positive electrode material obtained by the present invention has a high degree of crystallization and compaction density, a high volume energy density and a small degree of influence on conductivity, which is specifically manifested in that the first discharge specific capacity at 0.1C is as high as 164.1 mAh·g -1 After 30 cycles, the 0.1C capacity retention rate was 98.8%. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Parameter diagram of lithium iron manganese phosphate positive electrode materials obtained in Example 1, Example 2, Example 3 and Comparative Example 1 and Comparative Example 2 of the present invention;

[0029] Figure 2 The first charge and discharge curve of the high specific energy lithium manganese iron phosphate positive electrode material of Example 2 of the present invention at 0.1C;

[0030] Figure 3 This is a cycle stability performance diagram of the high specific energy lithium manganese iron phosphate positive electrode material at 0.1C according to Example 2 of the present invention.

[0031] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0034] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0035] Embodiment 1: This embodiment provides a method for preparing a high specific energy lithium manganese iron phosphate positive electrode material, and the specific steps are as follows:

[0036] S1. Prepare the raw materials required for preparing high specific energy lithium manganese iron phosphate positive electrode material: manganese source, iron source, lithium source, phosphoric acid source, dysprosium sulfate, polyvinyl alcohol, sodium caseinate, polyvinyl pyrrolidone, styrene, azobisisobutyramidine hydrochloride, ethanol, N,N-dimethylformamide, deionized water;

[0037] S2. 82.78 g of manganese phosphate, 45.25 g of iron orthophosphate, 36.95 g of lithium carbonate, and 22.86 g of phosphoric acid were weighed and mixed to obtain a mixture 1. Dysprosium sulfate was weighed according to 3% of the mass of the mixture 1, and the dysprosium sulfate was mixed with the mixture 1 and dispersed uniformly. The mixture was sintered at a high temperature of 500 ° C under a nitrogen atmosphere, and naturally cooled to room temperature. After crushing, a powder 1 with a particle size of 6 μm was obtained;

[0038] S3. Powder 1, sodium caseinate and polyvinyl alcohol obtained in step S2 are weighed in a mass ratio of 1:0.06:0.08, and mixture 2 is obtained after mixing. Deionized water of 15 times the mass of mixture 2 is added, and then stirring is continued at 90°C for 20 minutes to obtain a gel-like substance. The gel-like substance is heated to 250°C for 2 hours under a nitrogen atmosphere, and then ground after completion, and then calcined at high temperature under a nitrogen atmosphere, and continuously treated at 500°C for 4 hours to obtain powder 2;

[0039] S4. Preparation of polystyrene microsphere powder: polyvinyl pyrrolidone, deionized water and styrene are weighed in a mass volume ratio of 0.1:120:6 (g:mL), polyvinyl pyrrolidone and deionized water are stirred evenly in a three-necked flask, styrene is added after nitrogen is passed for 45 minutes, and stirring is continued at 100 rpm for 15 minutes to obtain liquid 1; liquid 1, azobisisobutyramidine hydrochloride and deionized water are weighed in a mass volume ratio of 10:0.1:20 (g:mL), liquid 1, azobisisobutyramidine hydrochloride and deionized water are mixed under a nitrogen atmosphere, and the reaction is continued at 80 rpm at 75°C for 30 hours, and then filtered, washed with ethanol and dried in an oven to obtain polystyrene microsphere powder.

[0040] S5. Weigh the powder 2 obtained in step S3, the polystyrene microsphere powder obtained in step S4 and N,N-dimethylformamide in a mass ratio of 1:0.1:8, mix them evenly to obtain a mixture 3, place the mixture 3 in a water bath, set the temperature to 50° C., and continue stirring for 4 hours to obtain a spinning solution;

[0041] S6. Inject the spinning solution obtained in step S5 into a 10mL plastic syringe equipped with a 20G stainless steel needle, and then fix the syringe on a micro-injection pump, connect one end of the needle to the positive electrode of a high-voltage electrostatic generator, and connect the collecting device to the negative electrode of the high-voltage electrostatic generator to perform electrostatic spinning to obtain precursor fibers; place the precursor fibers at room temperature for 12 hours, and then transfer them to a tubular sintering furnace, first pre-oxidize them at 180°C in air for 4 hours, and then keep them warm at 680°C in an argon-hydrogen mixed atmosphere for 2 hours to obtain a high-energy lithium iron manganese phosphate positive electrode material.

[0042] Embodiment 2: This embodiment provides a method for preparing a high specific energy lithium manganese iron phosphate positive electrode material, and the specific steps are as follows:

[0043] S1. Prepare the raw materials required for preparing high specific energy lithium manganese iron phosphate positive electrode material: manganese source, iron source, lithium source, phosphoric acid source, dysprosium sulfate, polyvinyl alcohol, sodium caseinate, polyvinyl pyrrolidone, styrene, azobisisobutyramidine hydrochloride, ethanol, N,N-dimethylformamide, deionized water;

[0044] S2. Weigh 82.78 g of manganese phosphate, 45.25 g of iron orthophosphate, 36.95 g of lithium carbonate, and 22.86 g of phosphoric acid, and mix them to obtain a mixture 1. Weigh 4% of the mass of the mixture 1 with dysprosium sulfate, mix the dysprosium sulfate with the mixture 1 and disperse them uniformly, sinter at high temperature under a nitrogen atmosphere at a sintering temperature of 520° C., cool naturally to room temperature, and crush to obtain a powder 1 with a particle size of 7 μm;

[0045] S3. Powder 1, sodium caseinate and polyvinyl alcohol obtained in step S2 are weighed in a mass ratio of 1:0.08:0.1, and mixture 2 is obtained after mixing. Deionized water of 24 times the mass of mixture 2 is added, and then stirring is continued at 95° C. for 25 min to obtain a gel-like substance. The gel-like substance is heated to 280° C. for 2.5 h in a nitrogen atmosphere, and then ground and calcined at high temperature in a nitrogen atmosphere, and continuously treated at 550° C. for 4.5 h to obtain powder 2.

[0046] S4. Preparation of polystyrene microsphere powder: polyvinyl pyrrolidone, deionized water and styrene are weighed in a mass volume ratio of 0.1:140:7 (g:mL), polyvinyl pyrrolidone and deionized water are stirred evenly in a three-necked flask, styrene is added after nitrogen is passed for 50 minutes, and stirring is continued at a speed of 110 rpm for 18 minutes to obtain liquid 1; liquid 1, azobisisobutyramidine hydrochloride and deionized water are weighed in a mass volume ratio of 10:0.12:25 (g:mL), liquid 1, azobisisobutyramidine hydrochloride and deionized water are mixed under a nitrogen atmosphere, and the reaction is continued at a speed of 100 rpm at 80°C for 32 hours, and then filtered, washed with ethanol and dried in an oven to obtain polystyrene microsphere powder.

[0047] S5. Weigh the powder 2 obtained in step S3, the polystyrene microsphere powder obtained in step S4 and N,N-dimethylformamide in a mass ratio of 1:0.15:10, mix them evenly to obtain a mixture 3, place the mixture 3 in a water bath, set the temperature to 55° C., and continue stirring for 4.5 hours to obtain a spinning solution;

[0048] S6. Inject the spinning solution obtained in step S5 into a 10mL plastic syringe equipped with a 20G stainless steel needle, and then fix the syringe on a micro-injection pump, connect one end of the needle to the positive electrode of a high-voltage electrostatic generator, and connect the collecting device to the negative electrode of the high-voltage electrostatic generator to perform electrostatic spinning to obtain precursor fibers; place the precursor fibers at room temperature for 16 hours, and then transfer them to a tubular sintering furnace, first pre-oxidize them at 190°C in air for 4.5 hours, and then keep them warm at 700°C in an argon-hydrogen mixed atmosphere for 2.5 hours to obtain a high-energy lithium iron manganese phosphate positive electrode material.

[0049] Embodiment 3: This embodiment provides a method for preparing a high specific energy lithium manganese iron phosphate positive electrode material, and the specific steps are as follows:

[0050] S1. Prepare the raw materials required for preparing high specific energy lithium manganese iron phosphate positive electrode material: manganese source, iron source, lithium source, phosphoric acid source, dysprosium sulfate, polyvinyl alcohol, sodium caseinate, polyvinyl pyrrolidone, styrene, azobisisobutyramidine hydrochloride, ethanol, N,N-dimethylformamide, deionized water;

[0051] S2. Weigh 60.90 g of manganese dioxide, 45.25 g of iron orthophosphate, 36.95 g of lithium carbonate, and 68.58 g of phosphoric acid, and mix to obtain a mixture 1. Weigh 5% of the mass of the mixture 1 with dysprosium sulfate, mix the dysprosium sulfate with the mixture 1 and disperse it evenly, sinter at high temperature under a nitrogen atmosphere at a sintering temperature of 550 ° C, cool naturally to room temperature, and crush to obtain a powder 1 with a particle size of 8 μm;

[0052] S3. Powder 1, sodium caseinate and polyvinyl alcohol obtained in step S2 are weighed in a mass ratio of 1:0.1:0.12, and mixture 2 is obtained after mixing. Deionized water in an amount of 30 times the mass of mixture 2 is added, and then stirring is continued at 100° C. for 30 min to obtain a gel-like substance. The gel-like substance is heated to 300° C. for 3 h in a nitrogen atmosphere, and then ground after completion, and then calcined at high temperature in a nitrogen atmosphere, and continued to be treated at 600° C. for 5 h to obtain powder 2;

[0053] S4. Preparation of polystyrene microsphere powder: polyvinyl pyrrolidone, deionized water and styrene are weighed in a mass-volume ratio of 0.1:150:8 (g:mL), polyvinyl pyrrolidone and deionized water are stirred evenly in a three-necked flask, styrene is added after nitrogen is passed for 60 minutes, and stirring is continued at 120 rpm for 20 minutes to obtain liquid 1; liquid 1, azobisisobutyramidine hydrochloride and deionized water are weighed in a mass-volume ratio of 10:0.15:30 (g:mL), liquid 1, azobisisobutyramidine hydrochloride and deionized water are mixed under a nitrogen atmosphere, and the reaction is continued at 85°C for 36 hours at a rotation speed of 120 rpm, and then filtered, washed with ethanol and dried in an oven to obtain polystyrene microsphere powder.

[0054] S5. Weigh the powder 2 obtained in step S3, the polystyrene microsphere powder obtained in step S4 and N,N-dimethylformamide in a mass ratio of 1:0.2:15, mix them evenly to obtain a mixture 3, place the mixture 3 in a water bath, set the temperature to 60° C., and continue stirring for 5 hours to obtain a spinning solution;

[0055] S6. The spinning solution obtained in step S5 is injected into a 10 mL plastic syringe equipped with a 20G stainless steel needle, and then the syringe is fixed on a micro-injection pump, one end of the needle is connected to the positive electrode of a high-voltage electrostatic generator, and the collecting device is connected to the negative electrode of the high-voltage electrostatic generator, and an electrostatic spinning operation is performed to obtain a precursor fiber; the precursor fiber is placed at room temperature for 20 hours, and then transferred to a tubular sintering furnace, first pre-oxidized at 200°C in air for 5 hours, and then kept warm at 720°C in an argon-hydrogen mixed atmosphere for 3 hours to obtain a high specific energy lithium manganese iron phosphate positive electrode material.

[0056] Comparative Example 1: This comparative example provides a method for preparing a lithium manganese iron phosphate positive electrode material, and the specific steps are as follows:

[0057] Weigh 82.78g of manganese phosphate, 45.25g of ferric orthophosphate, 36.95g of lithium carbonate, and 22.86g of phosphoric acid, and mix to obtain mixture 1, weigh 8% of glucose in mixture 1 by mass, weigh 10% of polyvinyl alcohol in mixture 1 by mass, and mix to obtain mixture 2, add 24 times the mass of deionized water in mixture 2, and then continue stirring at 95°C for 25min to obtain mixture 3, heat mixture 3 to 280°C under a nitrogen atmosphere for 2.5h, grind it after completion, and then calcine it at high temperature under a nitrogen atmosphere, and continue treating at 550°C for 4.5h to obtain the lithium iron manganese phosphate positive electrode material of this comparative example.

[0058] Comparative Example 2: This comparative example provides a method for preparing a lithium manganese iron phosphate positive electrode material, and the specific steps are as follows:

[0059] The difference between this comparative example and comparative example 1 is that after obtaining mixture 2, deionized water twice the mass of mixture 2 is added, poured into a spray dryer, the air inlet temperature is set to 230°C, and the air outlet temperature is set to 120°C, and then the obtained dry powder is transferred to a tubular sintering furnace, sintered for 6 hours in a nitrogen atmosphere at 700°C, naturally cooled to room temperature, and crushed to obtain lithium manganese iron phosphate positive electrode material.

[0060] Experimental test:

[0061] 1. The steps for testing the conductivity of the lithium iron manganese phosphate positive electrode materials obtained in Examples 1, 2, 3 of the present invention and Comparative Examples 1 and 2 are as follows:

[0062] Place the cathode material powder on the tablet press, apply a pressure of 10 MPa, maintain the pressure for 1 minute, measure the resistance, release the pressure, and finally measure the mold height. Use the formula σ=[4(L2–L1)] / πd 2 R is used to calculate the electrical conductivity of the powder (σ, S / cm), where L1 represents the original height of the mold, cm; L2 represents the height of the mold after compaction, cm; D represents the radius of the mold, cm; and R represents the resistance, Ω.

[0063] 2. The specific surface areas of the lithium iron manganese phosphate positive electrode materials obtained in Examples 1, 2, 3 of the present invention and Comparative Examples 1 and 2 were measured using a static nitrogen adsorption instrument (WBL-830, Zhejiang Sai De Instrument).

[0064] 3. The compaction density test steps of the lithium iron manganese phosphate positive electrode materials obtained in Examples 1, 2, 3 of the present invention and Comparative Examples 1 and 2 are as follows:

[0065] The crushed positive electrode material powder is coated on aluminum foil and then measured and calculated after being rolled. First, the relevant parameters of the electrode are measured, according to the formula ρ s =(m j -m l ) / S calculates the surface density of the pole piece (ρ s , g / cm 2 ), where m j Indicates the mass of the electrode, g; m l Indicates the mass of aluminum foil, g; S indicates the area of ​​the electrode, cm 2 .

[0066] Measure the thickness of the pole piece and aluminum foil after the roller, and after the unit conversion is completed, according to the formula ρ y =ρ s / (h j -h l )Calculate the compacted density (ρ y , g / cm 3 ), where ρ srepresents the surface density, g cm -2 ;h j Indicates the thickness of the electrode, cm; h l Indicates the thickness of the aluminum foil, cm.

[0067] 4. The test steps of the first charge and discharge curve and cycle stability performance diagram of the high specific energy lithium manganese iron phosphate positive electrode material at 0.1C in Example 2 of the present invention are as follows:

[0068] The charging and discharging mode adopted is: first constant current charging, then constant voltage charging for 2h, and finally constant current discharging. The charging and discharging cut-off voltage is: 2.5-4.5V. The rate test is carried out at 0.1C (1C = 170mAh·g -1 ) rates for 5 cycles respectively. During the cycle test, the battery was first activated at 0.1C rate for three cycles, and then the charge and discharge tests at other rates were performed. The test temperature was room temperature.

[0069] Result analysis:

[0070] Figure 1 The parameters of the lithium iron manganese phosphate positive electrode materials obtained in Examples 1, 2, and 3 of the present invention and Comparative Examples 1 and 2 are shown. It can be seen that compared with Comparative Examples 1 and 2, the lithium iron manganese phosphate positive electrode materials prepared in Examples 1-3 have higher compaction density, that is, higher volume energy density. Due to the addition of rare earth elements, the lithium iron manganese phosphate positive electrode materials prepared in Examples 1-3 also have higher specific surface areas and the same electrical conductivity.

[0071] Figure 2 This is the first charge and discharge curve of the high specific energy lithium manganese iron phosphate positive electrode material of Example 2 of the present invention at 0.1C. It can be observed that its first discharge specific capacity at 0.1C is as high as 164.1 mAh·g -1 , with high specific energy.

[0072] Figure 3 This is a cycle stability performance diagram of the high specific energy lithium manganese iron phosphate positive electrode material of Example 2 of the present invention at 0.1C. It can be observed that after 30 cycles, the 0.1C capacity retention rate is 98.8%, and the electrochemical performance is excellent and stable.

[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0074] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A high specific energy lithium manganese iron phosphate positive electrode material, characterized in that: The general chemical formula of the high specific energy lithium manganese iron phosphate positive electrode material is LiMn x Fe 1-x PO4@Dy / C / PS, x ranges from 0.6 to 0.8, Dy represents the rare earth element dysprosium, C represents the carbon source, specifically polyvinyl alcohol and sodium caseinate, and PS represents polystyrene microspheres.

2. The high specific energy lithium iron manganese phosphate positive electrode material according to claim 1, characterized in that: The general chemical formula of the high specific energy lithium manganese iron phosphate positive electrode material is LiMn x Fe 1-x PO4@Dy / C / PS, the value of x is 0.

7.

3. A method for preparing a high specific energy lithium manganese iron phosphate positive electrode material according to claim 1 or 2, characterized in that: The specific steps include: S1. Prepare the raw materials required for preparing high specific energy lithium manganese iron phosphate positive electrode material; S2. Weigh the corresponding mass fractions of manganese source, iron source, lithium source and phosphate source according to the atomic ratio, mix them to obtain mixture 1, weigh dysprosium sulfate according to 3%-5% of the mass of mixture 1, mix dysprosium sulfate with mixture 1 and disperse them evenly, sinter at high temperature, cool naturally to room temperature, and crush to obtain powder 1; S3. The powder 1, sodium caseinate and polyvinyl alcohol obtained in step S2 are weighed in a mass ratio of 1:0.06-0.1:0.08-0.12, and the mixture is mixed to obtain a mixture 2, and 15-30 times the mass of deionized water of the mixture 2 is added, and then heated and stirred to obtain a gel-like substance, and the gel-like substance is heated under a nitrogen atmosphere, and then ground and calcined at a high temperature to obtain a powder 2; S4. Preparation of polystyrene microsphere powder; S5. The powder 2 obtained in step S3, the polystyrene microsphere powder obtained in step S4 and N,N-dimethylformamide are weighed in a mass ratio of 1:0.1-0.2:8-15, and the mixture 3 is obtained after being mixed evenly. The mixture 3 is placed in a water bath, heated and continuously stirred to obtain a spinning solution; S6. The spinning solution obtained in step S5 is made into a precursor fiber by electrospinning technology, and then pre-oxidized and heat-treated in sequence to obtain a high specific energy lithium manganese iron phosphate cathode material; In step S1, the raw materials include the following substances: manganese source, iron source, lithium source, phosphate source, dysprosium sulfate, polyvinyl alcohol, sodium caseinate, polyvinyl pyrrolidone, styrene, azobisisobutyramidine hydrochloride, ethanol, N,N-dimethylformamide, and deionized water; The manganese source is preferably manganese phosphate or manganese dioxide, the iron source is preferably ferric orthophosphate, the lithium source is preferably lithium carbonate, the phosphoric acid source is provided by manganese phosphate and ferric orthophosphate, and the insufficient part is made up by phosphoric acid.

4. A method for preparing the high specific energy lithium manganese iron phosphate positive electrode material according to claim 3, characterized in that: In step S4, the following steps are specifically included: S4.

1. Weigh polyvinyl pyrrolidone, deionized water, and styrene in a mass-to-volume ratio of 0.1:120-150:6-8, stir the polyvinyl pyrrolidone and deionized water in a three-necked flask, add styrene after nitrogen is passed, and continue stirring to obtain liquid 1; S4.

2. Weigh liquid 1, azobisisobutylamidine hydrochloride, and deionized water in a mass-to-volume ratio of 10:0.1-0.15:20-30, mix liquid 1, azobisisobutylamidine hydrochloride, and deionized water under a nitrogen atmosphere, heat and stir to continue the reaction, then filter, wash with ethanol, and dry in an oven to obtain polystyrene microsphere powder.

5. A method for preparing the high specific energy lithium manganese iron phosphate positive electrode material according to claim 3, characterized in that: In step S6, the following steps are specifically included: S6.1, injecting the spinning solution obtained in step S5 into a plastic syringe equipped with a 20G stainless steel needle, and then fixing the syringe on a micro-injection pump, connecting one end of the needle to the positive electrode of a high-voltage electrostatic generator, and connecting a collecting device to the negative electrode of the high-voltage electrostatic generator, and performing an electrospinning operation to obtain a precursor fiber; S6.

2. Place the precursor fiber in step S6.1 at room temperature for 12-20 hours, then transfer it to a tubular sintering furnace, pre-oxidize it in air, and then keep it warm for 2-3 hours in an argon-hydrogen mixed atmosphere to obtain a high-energy lithium manganese iron phosphate positive electrode material.

Citation Information

Patent Citations

  • Preparation method of positive electrode material LiFePO4 / C of lithium ion battery

    CN101950801A

  • Preparation method of carbon-coated lithium iron phosphate material with polystyrene microspheres and polyethylene glycol as carbon sources

    CN103346323A

  • A positive electrode material of a lithium ion battery with a coating layer and a preparation method thereof

    CN108987727A

  • Method and device for preparing lithium iron manganese phosphate fiber positive electrode material

    CN114975952A

  • Method for preparing composite nanofiber membrane with embedded hollow titanium dioxide balls through electrostatic spinning

    CN116065302A