Micron silicon negative electrode material and preparation method thereof, lithium ion battery and electric equipment
By premodifying the surface hydroxyl group and polymer coating on the micron silicon powder, the SiOx@PC coating is formed, which solves the structural stability and cycle life of the micron silicon-based anode material in lithium-ion batteries, and achieves low expansion and micron silicon anode material with high electrochemical properties.
Patent Information
- Application Number
- CN202411085757.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
The existing micron silicon-based anode materials are prone to structural crushing and volume changes during the electrochemical lithiation/delithiation cycle, resulting in disconnection of electron transport paths and consumption of solid electrolyte interphase layer, and the existing carbon coating is difficult to compatible with micron silicon. The irregular size and volume changes of particles cannot effectively suppress expansion and improve cycle life.
By pre-modifying the surface hydroxyl group of micron silicon powder, mixing it with ethanol and polyethylene glycol, adding a carboxyl-containing polymer solution to form a hybrid hydrogel, and after drying and high-temperature heat treatment, silicon oxide coated micron silicon is formed. The core-shell structure of the core and ultra-thin carbon shell forms a SiOx@PC coating to alleviate volume expansion and improve electrochemical performance.
The low expansion and long cycle life of micron silicon anode material in lithium-ion batteries is achieved, which significantly improves the kinetic performance and mechanical stability of the electrochemical reaction, improves the electrochemical cycle stability and reduces the expansion rate.
Smart Images

Figure CN118983422A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of micron-sized silicon-based negative electrode materials, and in particular to a micron silicon negative electrode material and a preparation method thereof, a lithium-ion battery and electrical equipment. Background Art
[0002] Silicon (Si) is considered to be an advanced alternative to graphite anodes because of its higher mass specific capacity (Li 3.75 Si, ~3579mAh g -1 ) and volumetric capacity (>2000mAh cm -3 ); and, compared with nano silicon powder, micron silicon powder has lower cost and higher packing density; in particular, micron silicon powder has a smaller specific surface area, which will largely avoid interface problems such as electrolyte decomposition and thermal risks in the battery.
[0003] However, micron / submicron silicon powder with a particle size greater than 150 nm will undergo structural crushing during the electrochemical lithiation / delithiation cycle, which will lead to the disconnection of the transmission path in the overall structure of electrons and the continuous consumption of the solid electrolyte interphase (SEI); although self-healing adhesives or electrolyte designs have been used to maintain the integrity of micron silicon particles to improve their cycling performance, their role in stabilizing the SEI layer is still very limited and cannot withstand the repeated volume changes of silicon particles during long cycle life.
[0004] In addition, another way to alleviate further cracking of silicon particles is to use high-quality carbon coatings to retain voids on the surface of micron silicon particles; however, in actual cycling, the carbon coating is easily broken because it is actually difficult for the rigid carbon layer to maintain an appropriate void volume compatible with irregular-sized and anisotropic micron silicon particles; therefore, when the volume changes drastically, cracks are very likely to occur, leading to failure of the entire electrode; and in the electrode preparation process, the micro-sized voids between the carbon shell and the micron silicon particles are difficult to withstand high-intensity pressure, and the carbon encapsulation reported earlier cannot simultaneously meet the strict requirements of manufacturing and cycling processes.
[0005] In the existing preparation of micron silicon-based negative electrode materials, there is a lack of structural design and production methods that can both inhibit the volume expansion of micron silicon particles and improve the electrochemical cycle life of micron silicon.
[0006] Therefore, the development of micron silicon-based materials with low expansion and long cycle life is an important direction for the large-scale application of silicon-carbon negative electrode materials in the field of lithium-ion battery negative electrodes. Summary of the invention
[0007] The purpose of this application is to provide a micron silicon negative electrode material and a preparation method thereof, a lithium ion battery and electrical equipment to solve the above problems.
[0008] To achieve the above objectives, the present application provides a first aspect of a method for preparing a micron silicon negative electrode material, comprising:
[0009] Performing surface hydroxyl pre-modification treatment on micron silicon powder to obtain surface hydroxyl modified micron silicon powder;
[0010] The surface hydroxyl-modified micron silicon powder, ethanol and polyethylene glycol are first mixed to obtain a first mixed solution;
[0011] performing a second mixing of the first mixed solution and the carboxyl group-containing polymer solution to obtain a second mixed solution;
[0012] heating the second mixed solution to obtain a hybrid hydrogel, and drying the hybrid hydrogel to obtain a hybrid silicon composite;
[0013] The hybrid silicon composite is subjected to high-temperature heat treatment to obtain the micron silicon negative electrode material.
[0014] Optionally, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0015] A. The micron silicon powder is obtained by crushing and screening industrial silicon powder;
[0016] B. The particle size of the micron silicon powder is 2 μm-10 μm.
[0017] Optionally, the surface hydroxyl pre-modification treatment comprises:
[0018] The micron silicon powder is refluxed and stirred in a lithium hydroxide solution, solid-liquid separation is performed to obtain a solid phase, and the solid phase is washed to obtain the micron silicon powder with surface hydroxyl groups modified.
[0019] Optionally, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0020] A. The concentration of the lithium hydroxide solution is 2 mol / L-5 mol / L, and the mass ratio of the micron silicon powder to the lithium hydroxide solution is (1-2): (1-5);
[0021] B. The washing detergent includes an acetic acid solution, and the concentration of the acetic acid solution is 1 mol / L-5 mol / L.
[0022] Optionally, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0023] A. the molecular weight of the polyethylene glycol is 300-500;
[0024] B. performing a first stirring after the first mixing, wherein the first stirring time is 2h-3h;
[0025] C. The mass ratio of the micron silicon powder, the ethanol and the polyethylene glycol in the first mixture is 1:(2-20):(1-15).
[0026] Optionally, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0027] A. The second mixing is carried out in a sand mill, the speed of the sand mill is 300r / min-400r / min, and the running time is 10min-15min;
[0028] B. the carboxyl-containing polymer solution comprises one or more of a polyacrylic acid solution, an acrylic acid-hydroxypropyl acrylate copolymer solution and an acrylic acid-acrylate copolymer solution;
[0029] C. the mass ratio of the first mixed solution to the carboxyl group-containing polymer solution in the second mixed solution is (1-10): 1;
[0030] D. The mass content of the carboxyl group-containing polymer solution is 5%-20%.
[0031] Optionally, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0032] A. The heating temperature is 120°C-180°C and the heating time is 2h-5h;
[0033] B. The drying adopts capillary drying technology, and the drying temperature is 60°C-90°C and the drying time is 24h-48h under normal pressure atmosphere.
[0034] C. The temperature of the high temperature heat treatment is 900°C-1100°C, and the time is 3h-5h.
[0035] The second aspect of the present application provides a micron silicon negative electrode material, which is prepared by the preparation method of the micron silicon negative electrode material.
[0036] The third aspect of the present application provides a lithium-ion battery, comprising the micron silicon negative electrode material.
[0037] A fourth aspect of the present application provides an electrical device, including the lithium-ion battery.
[0038] Compared with the prior art, the beneficial effects of this application include:
[0039] The preparation method of micron silicon negative electrode material provided in the present application selects micron silicon powder as raw material. Compared with nano silicon powder, micron silicon powder is cheap and widely available, and its higher packing density is more conducive to improving the overall energy density of the battery end; the micron silicon powder is subjected to surface hydroxyl pre-modification treatment, first mixing and second mixing to obtain a stable composite tightly bound by hydroxyl-carboxyl-hydroxyl intermolecular hydrogen bonding force, wherein the stable composite can form intermolecular hydrogen bonding with the silicon surface hydroxyl group through the carboxyl group in the carboxyl-containing polymer and then adsorb each other to form a core-shell coating structure, and then the micron silicon negative electrode material is prepared by high-temperature heat treatment. The preparation method is suitable for large-scale industrial production.
[0040] The micron silicon negative electrode material (MSi-SiO x @PC), made of silicon oxide (SiO x ) is composed of a core structure of micron silicon (MSi) and an ultra-thin highly conductive carbon shell structure (PC), wherein silicon dioxide is used as a buffer matrix, considering its elastic properties and its close bonding with silicon, and amorphous SiO x The volume expansion is small, so the volume expansion of silicon can be effectively alleviated during the cycle. In addition, SiO x @PC coating not only helps to release the stress of adapting to volume change, but also accelerates Li + Rapid transfer from the outer shell to the inner silicon core is based on the in-situ formation of SiO between PC and MSi. x The interlayer can effectively reduce Li + Energy barrier for transport from PC to MSi; SiO x @PC coating provides a fast mixing pathway for ions and electrons, which helps to enhance the MSi-SiO x @PC micron silicon negative electrode material electrochemical reaction kinetics, thereby maintaining mechanical stability of volume change; this is due to the high modulus SiO x @PC helps to release stress during lithiation and delithiation, thus, SiO x @ PC activated Li + The path can remain stable even when volume changes occur; the electrochemical cycle stability of micron-sized silicon powder is greatly improved and the expansion rate during lithiation is significantly reduced through reasonable surface and interface structure design; the micron silicon negative electrode material provided in the present application has significantly improved electrochemical cycle performance without obvious capacity change differences, and the micron silicon negative electrode material can play a major role in promoting the use of micro silicon in micron silicon-carbon negative electrodes for lithium-ion batteries.
[0041] The lithium-ion battery and electrical equipment provided in this application have excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0043] Figure 1 This is a SEM image of the industrial silicon powder used in the examples and comparative examples of the present application;
[0044] Figure 2 The MSi-SiO prepared in Example 1 X @SEM image of PC1;
[0045] Figure 3 The MSi-SiO prepared in Example 1 X @XPS pattern of Si 2p of PC1;
[0046] Figure 4 The MSi-SiO prepared in Example 1 X @PC1’s electrochemical cycle test diagram with industrial silicon powder. DETAILED DESCRIPTION
[0047] As used herein:
[0048] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0049] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0050] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0051] In these examples, parts and percentages are by mass unless otherwise indicated.
[0052] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0053] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0054] The first aspect of the present application provides a method for preparing a micron silicon negative electrode material, comprising:
[0055] Performing surface hydroxyl pre-modification treatment on micron silicon powder to obtain surface hydroxyl modified micron silicon powder;
[0056] The surface hydroxyl-modified micron silicon powder, ethanol and polyethylene glycol are first mixed to obtain a first mixed solution;
[0057] performing a second mixing of the first mixed solution and the carboxyl group-containing polymer solution to obtain a second mixed solution;
[0058] heating the second mixed solution to obtain a hybrid hydrogel, and drying the hybrid hydrogel to obtain a hybrid silicon composite;
[0059] The hybrid silicon composite is subjected to high-temperature heat treatment to obtain the micron silicon negative electrode material.
[0060] In some embodiments, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0061] A. The micron silicon powder is obtained by crushing and screening industrial silicon powder;
[0062] B. The particle size of the micron silicon powder is 2 μm-10 μm.
[0063] Optionally, the particle size of the micron silicon powder may be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm or any value between 2 μm and 10 μm.
[0064] It should be noted that micron silicon powder with a particle size greater than 10 μm is easy to settle in the water phase, while micron silicon powder with a particle size less than 2 μm is easy to aggregate and difficult to disperse in the water phase.
[0065] In some embodiments, the surface hydroxyl pre-modification treatment comprises:
[0066] The micron silicon powder is refluxed and stirred in a lithium hydroxide solution, solid-liquid separation is performed to obtain a solid phase, and the solid phase is washed to obtain the micron silicon powder with surface hydroxyl groups modified.
[0067] It should be noted that the micron silicon powder is refluxed and stirred in a lithium hydroxide solution. Lithium hydroxide is a hydroxyl-rich inorganic substance. The hydroxyl groups produced by the decomposition of its aqueous solution under reflux are easy to hydroxylate the surface of the micron silicon powder. In addition, considering that similar inorganic hydroxyl salts, such as sodium hydroxide, have stronger alkalinity and will have higher requirements on experimental equipment, lithium hydroxide is selected as the inorganic salt used for silicon-based hydroxylation.
[0068] In some embodiments, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0069] A. The concentration of the lithium hydroxide solution is 2 mol / L-5 mol / L, and the mass ratio of the micron silicon powder to the lithium hydroxide solution is (1-2): (1-5);
[0070] Optionally, the concentration of the lithium hydroxide solution may be 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L or any value between 2 mol / L and 5 mol / L, and the mass ratio of the micron silicon powder to the lithium hydroxide solution may be 1:1, 1:2, 1:3, 1:4, 1:5, 2:1, 2:3, 2:4, 2:5 or any value between (1-2):(1-5);
[0071] B. The washing detergent includes an acetic acid solution, and the concentration of the acetic acid solution is 1 mol / L-5 mol / L.
[0072] Optionally, the concentration of the acetic acid solution may be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L or any value between 1 mol / L and 5 mol / L.
[0073] It should be noted that the detergent includes an acetic acid solution, which can neutralize some of the unreacted hydroxide ions and will not produce side reactions on the surface of the hydroxylated silicon.
[0074] In some embodiments, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0075] A. the molecular weight of the polyethylene glycol is 300-500;
[0076] Optionally, the molecular weight of polyethylene glycol is 300, 350, 400, 450, 500 or any value between 300 and 500;
[0077] It should be noted that when the molecular weight of polyethylene glycol is 300-500, it is liquid at room temperature, while polyethylene glycol with a molecular weight above 600 gradually becomes semi-solid or even solid.
[0078] B. performing a first stirring after the first mixing, wherein the first stirring time is 2h-3h;
[0079] Optionally, the first stirring time can be 2h, 2.5h, 3h or any value between 2h and 3h;
[0080] C. The mass ratio of the micron silicon powder, the ethanol and the polyethylene glycol in the first mixture is 1:(2-20):(1-15).
[0081] Optionally, the mass ratio of micron silicon powder, ethanol and polyethylene glycol in the first mixture can be 1:2:1, 1:5:1, 1:10:1, 1:15:1, 1:20:1, 1:2:5, 1:2:10, 1:2:15 or any value between 1:(2-20):(1-15).
[0082] Preferably, the first mixing comprises mixing micron silicon powder and ethanol to obtain a micron silicon powder ethanol mixed solution, and mixing the micron silicon powder ethanol mixed solution and an ethanol solution of polyethylene glycol to obtain a first mixed solution.
[0083] It should be noted that the micron silicon powder and ethanol are first mixed to obtain a micron silicon powder ethanol mixed solution, and then the micron silicon powder ethanol mixed solution is mixed with an ethanol solution of polyethylene glycol. The micron silicon powder has better dispersibility in the ethanol solution, and the effect of adding polyethylene glycol for thickening treatment is better.
[0084] In some embodiments, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0085] A. The second mixing is carried out in a sand mill, the speed of the sand mill is 300r / min-400r / min, and the running time is 10min-15min;
[0086] Optionally, the speed of the sand mill can be 300r / min, 320r / min, 340r / min, 360r / min, 380r / min, 400r / min or any value between 300r / min-400r / min, and the running time can be 10min, 11min, 12min, 13min, 14min, 15min or any value between 10min-15min;
[0087] It should be noted that the second mixing is carried out in a sand mill. The introduction of gradient-sized zirconium beads in the sand mill will make the contact between different phases in the dispersion more complete, and the stirring effect will significantly optimize the traditional stirring bar stirring and mechanical rod stirring.
[0088] B. the carboxyl-containing polymer solution comprises one or more of a polyacrylic acid solution, an acrylic acid-hydroxypropyl acrylate copolymer solution and an acrylic acid-acrylate copolymer solution;
[0089] It should be noted that the carboxyl-containing polymer solution includes one or more of polyacrylic acid solution, acrylic acid-hydroxypropyl acrylate copolymer solution and acrylic acid-acrylate copolymer solution, and the above three carboxyl polymer solutions are carboxyl-rich linear polymers, in which the carboxyl group and the hydroxyl group on the silicon surface can form intermolecular hydrogen bonds and then adsorb each other to form a core-shell coating structure; and the liquid state of the above three carboxyl polymers at room temperature is more beneficial to the coating of the solid dispersed phase of microsilica powder in the liquid phase; in addition, polyacrylic acid and its derivative polymers will form a carbon layer structure with excellent electrical conductivity after heat treatment, thereby improving the electrical conductivity of the microsilica powder.
[0090] It should also be noted that the main difference between the above three carboxyl polymer solutions is that polyacrylic acid has the highest carboxyl content, followed by acrylic acid-acrylate, and acrylic acid-hydroxypropyl acrylate has the lowest carboxyl content compared to the above two; it should be noted that, due to the low electrical conductivity of the silicon powder material itself, the introduction of carboxyl polymers will form a carbon layer structure with excellent electrical conductivity after heat treatment, thereby improving the electrical conductivity of the microsilica powder.
[0091] C. the mass ratio of the first mixed solution to the carboxyl group-containing polymer in the second mixed solution is (1-10): 1;
[0092] Optionally, the mass ratio of the first mixed solution to the carboxyl-containing polymer in the second mixture can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or any value between (1-10):1;
[0093] D. The mass content of the carboxyl group-containing polymer solution is 5%-20%.
[0094] Optionally, the mass content of the carboxyl-containing polymer solution may be 5%, 10%, 15%, 20% or any value between 5% and 20%.
[0095] In some embodiments, the method for preparing the micron silicon negative electrode material satisfies at least one of the following conditions:
[0096] A. The heating temperature is 120°C-180°C and the heating time is 2h-5h;
[0097] Optionally, the heating temperature may be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or any value between 120°C and 180°C, and the heating time may be 2h, 3h, 4h, 5h or any value between 2h and 5h;
[0098] B. The drying adopts capillary drying technology, and the drying temperature is 60°C-90°C and the drying time is 24h-48h under normal pressure atmosphere;
[0099] Optionally, the drying temperature may be 60°C, 70°C, 80°C, 90°C or any value between 60°C and 90°C, and the drying time may be 24h, 28h, 32h, 36h, 40h, 44h, 48h or any value between 24h and 48h;
[0100] It should be noted that during the drying process of powder materials dispersed in the liquid phase, material agglomeration or powder accumulation to varying degrees usually occurs. The use of capillary drying technology can avoid the powder accumulation caused by the sample drying process, thereby optimizing the packing density of the powder material.
[0101] C. The temperature of the high temperature heat treatment is 900°C-1100°C, and the time is 3h-5h.
[0102] Optionally, the temperature of the high-temperature heat treatment can be 900°C, 950°C, 1000°C, 1050°C, 1100°C or any value between 900°C and 1100°C, and the time of the high-temperature heat treatment can be 3h, 4h, 5h or any value between 3h and 5h.
[0103] The second aspect of the present application provides a micron silicon negative electrode material, which is prepared by the preparation method of the micron silicon negative electrode material.
[0104] The third aspect of the present application provides a lithium-ion battery, comprising the micron silicon negative electrode material.
[0105] A fourth aspect of the present application provides an electrical device, including the lithium-ion battery.
[0106] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0107] The industrial silicon powder used in the examples and comparative examples of this application is common commercially available photovoltaic silicon waste. The SEM images of the industrial silicon powder are as follows: Figure 1 shown.
[0108] Example 1
[0109] A first aspect of this embodiment provides a method for preparing a micron silicon negative electrode material, comprising:
[0110] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0111] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0112] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0113] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of polyacrylic acid (PAA) (mass content 6%) is added, the mass ratio of the first mixed solution to the polyacrylic acid solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0114] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0115] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain a micron silicon negative electrode material MSi-SiO X @PC1.
[0116] The second aspect of this embodiment provides a micron silicon negative electrode material MSi-SiO X @PC1 was prepared by the above preparation method.
[0117] The micron silicon negative electrode material MSi-SiO X @PC1 SEM picture Figure 2 shown.
[0118] The micron silicon negative electrode material MSi-SiO X XPS of Si 2p @PC1 Figure 3 shown.
[0119] The micron silicon negative electrode material MSi-SiO X @PC1 and industrial silicon powder electrochemical cycle test Figure 4 shown.
[0120] Example 2
[0121] A first aspect of this embodiment provides a method for preparing a micron silicon negative electrode material, comprising:
[0122] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0123] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0124] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0125] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of acrylic acid-hydroxypropyl acrylate copolymer (AC) (mass content 6%) is added, the mass ratio of the first mixed solution to the acrylic acid-hydroxypropyl acrylate copolymer solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0126] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0127] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain a micron silicon negative electrode material MSi-SiO X @PC2.
[0128] The second aspect of this embodiment provides a micron silicon negative electrode material MSi-SiO X @PC2 was prepared by the above preparation method.
[0129] Example 3
[0130] A first aspect of this embodiment provides a method for preparing a micron silicon negative electrode material, comprising:
[0131] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0132] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0133] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0134] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of acrylic acid-acrylic acid ester copolymer (AA / HPA) (mass content 6%) is added, the mass ratio of the first mixed solution to the acrylic acid-acrylic acid ester copolymer solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0135] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0136] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain a micron silicon negative electrode material MSi-SiO X @PC3.
[0137] The second aspect of this embodiment provides a micron silicon negative electrode material MSi-SiO X @PC3, prepared by the above preparation method.
[0138] Comparative Example 1
[0139] The first aspect of this comparative example provides a method for preparing a micron silicon negative electrode material, which is different from Example 1 in that the mass content of polyacrylic acid (PAA) in this comparative example is 3%, and the specific steps are as follows:
[0140] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0141] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0142] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0143] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of polyacrylic acid (PAA) (mass content 3%) is added, the mass ratio of the first mixed solution to the polyacrylic acid solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0144] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0145] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain a micron silicon negative electrode material MSi-SiO X @PC4.
[0146] The second aspect of this comparative example provides a micron silicon negative electrode material MSi-SiO X @PC4 was prepared by the above preparation method.
[0147] Comparative Example 2
[0148] The first aspect of this comparative example provides a method for preparing a micron silicon negative electrode material, which is different from Example 1 in that the mass content of polyacrylic acid (PAA) in this comparative example is 12%, and the specific steps are as follows:
[0149] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0150] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0151] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0152] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of polyacrylic acid (PAA) (mass content 12%) is added, the mass ratio of the first mixed solution to the polyacrylic acid solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0153] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0154] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain a micron silicon negative electrode material MSi-SiO X @PC5.
[0155] The second aspect of this comparative example provides a micron silicon negative electrode material MSi-SiO X @PC5 was prepared by the above preparation method.
[0156] Comparative Example 3
[0157] The first aspect of this comparative example provides a method for preparing a micron silicon negative electrode material, which is different from Example 1 in that the temperature of the high-temperature heat treatment in this comparative example is 800° C., and the specific steps are as follows:
[0158] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0159] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0160] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0161] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of polyacrylic acid (PAA) (mass content 6%) is added, the mass ratio of the first mixed solution to the polyacrylic acid solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0162] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0163] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 800°C for 5 hours to obtain the micron silicon negative electrode material MSi-SiO X @PC6.
[0164] The second aspect of this comparative example provides a micron silicon negative electrode material MSi-SiO X @PC6 was prepared by the above preparation method.
[0165] Comparative Example 4
[0166] The first aspect of this comparative example provides a method for preparing a micron silicon negative electrode material, which is different from Example 1 in that the temperature of the high-temperature heat treatment in this comparative example is 900° C., and the specific steps are as follows:
[0167] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0168] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0169] S3: Dispersing the surface hydroxyl-modified micron silicon powder in an ethanol solution, stirring it fully for 2 hours at room temperature, and then adding a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and performing a first stirring after the first mixing, the first stirring time is 2.5 hours, to obtain a first mixed solution;
[0170] S4: the first mixed solution is transferred to a sand mill, and an ethanol solution of polyacrylic acid (PAA) (mass content 6%) is added, the mass ratio of the first mixed solution to the polyacrylic acid solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0171] S5: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0172] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 900°C for 5 hours to obtain the micron silicon negative electrode material MSi-SiO X @PC7.
[0173] The second aspect of this comparative example provides a micron silicon negative electrode material MSi-SiO X @PC7, prepared by the above preparation method.
[0174] Comparative Example 5
[0175] The first aspect of this comparative example provides a method for preparing a micron silicon negative electrode material, which is different from Example 1 in that the present comparative example does not perform a surface hydroxyl pre-modification treatment, and the specific steps are as follows:
[0176] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm (5μm);
[0177] S2: Disperse the micron silicon powder in an ethanol solution, stir it thoroughly for 2 hours at room temperature, then add a 400 molecular weight polyethylene glycol (mass content 15%) ethanol solution for thickening treatment, the mass ratio of the micron silicon powder, ethanol and polyethylene glycol is 1:10:4, and perform a first stirring after the first mixing, the first stirring time is 2.5 hours, and obtain a first mixed solution;
[0178] S3: the first mixed solution is transferred to a sand mill, and an ethanol solution of polyacrylic acid (PAA) (mass content 6%) is added, the mass ratio of the first mixed solution to the polyacrylic acid solution is 3:1, the speed of the sand mill is 350 r / min, the running time is 15 min, and the mixture is fully mixed to obtain a second mixed solution;
[0179] S4: heating the second mixed solution at 150° C. for 3 h to prepare a hybrid hydrogel, and treating the hybrid hydrogel by capillary drying technology in a normal pressure atmosphere at 70° C. for 36 h to obtain a hybrid silicon composite;
[0180] S5: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain the micron silicon negative electrode material MSi-SiO X @PC8.
[0181] The second aspect of this embodiment provides a micron silicon negative electrode material MSi-SiO X @PC8 was prepared by the above preparation method.
[0182] Comparative Example 6
[0183] The first aspect of this comparative example provides a method for preparing a micron silicon negative electrode material, which is different from Example 1 in that the first mixing and the second mixing treatments are not performed in this comparative example, and the specific steps are as follows:
[0184] S1: crush the common commercially available industrial silicon powder using a sand mill and classify it using an ultrasonic vibration sieving machine to obtain micron silicon powder with a particle size of 2μm-10μm;
[0185] S2: pre-modifying the surface of the micron silicon powder with hydroxyl groups, wherein the pre-modification of the surface hydroxyl groups comprises refluxing and stirring the micron silicon powder in a 2M lithium hydroxide solution for 4 hours, separating the solid from the liquid to obtain a solid phase, and washing the solid phase with a 3M acetic acid solution to obtain the surface hydroxyl-modified micron silicon powder;
[0186] S5: heating the surface hydroxyl-modified micron silicon powder at 150° C. for 3 h, and drying it at 70° C. for 36 h in a normal pressure atmosphere by capillary drying technology to obtain a hybrid silicon composite;
[0187] S6: Under nitrogen protection, the hybrid silicon composite is subjected to high temperature heat treatment at a temperature of 1050°C for 5 hours to obtain a micron silicon negative electrode material MSi-SiO X @PC9.
[0188] The second aspect of this comparative example provides a micron silicon negative electrode material MSi-SiO X @PC9 was prepared by the above preparation method.
[0189] The micron silicon negative electrode materials prepared in the above examples and comparative examples and the commercially available industrial silicon powder MSi were subjected to electrochemical performance tests and pole piece expansion tests. The specific test results are shown in Table 1.
[0190] Table 1 Electrochemical performance test and electrode expansion test
[0191]
[0192] Specific capacity test method: In button cells, the mass of silicon-based negative electrode materials is used as a benchmark, and the battery material capacity is calculated through a constant current charge and discharge test method. Specific capacity = material capacity / active material mass.
[0193] First-cycle efficiency test method: First-cycle efficiency mainly refers to the efficiency of the battery during the first discharge process, that is, the ratio of discharge capacity to charging capacity.
[0194] Cycle test method: The battery cycle test method is to perform multiple charge and discharge cycles on the battery to evaluate its performance and life. A cycle is the time from the start of the charging process to the end of the next week's discharge process.
[0195] Capacity retention rate test method: The ratio of the charging capacity under the corresponding number of cycles to the initial charging capacity is the capacity retention rate of the corresponding number of cycles.
[0196] Pole piece expansion rate (%) test method: The ratio of the pole piece thickness under the corresponding number of turns to the pole piece thickness after initialization is the pole piece expansion rate under the corresponding number of turns.
[0197] From the above test results, it can be seen that compared with Example 1, Example 1 has higher specific capacity, first cycle coulomb efficiency, higher capacity retention rate and lower pole piece expansion rate. This is mainly because the hydrogen bonding between polyacrylic acid with higher carboxyl content and hydroxyl-modified micron silicon leads to a more uniform coating effect, so that the in-situ coated carbon layer structure formed after heat treatment is more uniformly deposited on the surface of silicon powder to form a uniform and stable conductive carbon layer, thereby achieving efficient and stable charge and discharge stability, and effectively suppressing the expansion effect of micron silicon.
[0198] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0199] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing a micron silicon negative electrode material, characterized in that: include: Performing surface hydroxyl pre-modification treatment on micron silicon powder to obtain surface hydroxyl modified micron silicon powder; The surface hydroxyl-modified micron silicon powder, ethanol and polyethylene glycol are first mixed to obtain a first mixed solution; performing a second mixing of the first mixed solution and the carboxyl group-containing polymer solution to obtain a second mixed solution; heating the second mixed solution to obtain a hybrid hydrogel, and drying the hybrid hydrogel to obtain a hybrid silicon composite; The hybrid silicon composite is subjected to high-temperature heat treatment to obtain the micron silicon negative electrode material.
2. The method for preparing the micron silicon negative electrode material according to claim 1, characterized in that: At least one of the following conditions is met: A. The micron silicon powder is obtained by crushing and screening industrial silicon powder; B. The particle size of the micron silicon powder is 2 μm-10 μm.
3. The method for preparing the micron silicon negative electrode material according to claim 1, characterized in that: The surface hydroxyl pre-modification treatment comprises: The micron silicon powder is refluxed and stirred in a lithium hydroxide solution, solid-liquid separation is performed to obtain a solid phase, and the solid phase is washed to obtain the micron silicon powder with surface hydroxyl groups modified.
4. The method for preparing the micron silicon negative electrode material according to claim 3, characterized in that: At least one of the following conditions is met: A. The concentration of the lithium hydroxide solution is 2 mol / L-5 mol / L, and the mass ratio of the micron silicon powder to the lithium hydroxide solution is (1-2): (1-5); B. The washing detergent includes an acetic acid solution, and the concentration of the acetic acid solution is 1 mol / L-5 mol / L.
5. The method for preparing the micron silicon negative electrode material according to claim 1, characterized in that: At least one of the following conditions is met: A. the molecular weight of the polyethylene glycol is 300-500; B. performing a first stirring after the first mixing, wherein the first stirring time is 2h-3h; C. The mass ratio of the micron silicon powder, the ethanol and the polyethylene glycol in the first mixture is 1:(2-20):(1-15).
6. The method for preparing the micron silicon negative electrode material according to claim 1, characterized in that: At least one of the following conditions is met: A. The second mixing is carried out in a sand mill, the speed of the sand mill is 300r / min-400r / min, and the running time is 10min-15min; B. the carboxyl-containing polymer solution comprises one or more of a polyacrylic acid solution, an acrylic acid-hydroxypropyl acrylate copolymer solution and an acrylic acid-acrylate copolymer solution; C. the mass ratio of the first mixed solution to the carboxyl group-containing polymer solution in the second mixed solution is (1-10): 1; D. The mass content of the carboxyl group-containing polymer solution is 5%-20%.
7. The method for preparing the micron silicon negative electrode material according to any one of claims 1 to 6, characterized in that: At least one of the following conditions is met: A. The heating temperature is 120°C-180°C and the heating time is 2h-5h; B. The drying adopts capillary drying technology, and the drying temperature is 60°C-90°C and the drying time is 24h-48h under normal pressure atmosphere; C. The temperature of the high temperature heat treatment is 900°C-1100°C, and the time is 3h-5h.
8. A micron silicon negative electrode material, characterized in that: The micron silicon negative electrode material is prepared by the preparation method of the micron silicon negative electrode material according to any one of claims 1 to 7.
9. A lithium ion battery, characterized in that: Including the micron silicon negative electrode material as described in claim 8.
10. An electrical equipment, characterized in that: Includes the lithium ion battery as claimed in claim 9.
Citation Information
Cited By
Modified silicon negative electrode material, preparation method of modified silicon negative electrode material, negative electrode plate and battery
CN119742334A
Micro-silicon-based negative electrode material, micro-silicon-based negative electrode and preparation methods of micro-silicon-based negative electrode material and micro-silicon-based negative electrode
CN120261539A
A microsilicon-based anode material and its preparation method
CN123120711A