Multi-metal element composite phosphate sodium battery positive electrode material and preparation method thereof
Through simplified preparation method and multi-metal element composite technology, the problems of complex and high cost of polymetal element composite phosphoric acid/ferrophosphate sodium pyrophosphate electropositive electrode material in the prior art are solved, and the multi-metal with high working voltage and energy density are achieved The preparation of elemental composite sodium phosphate electropositive electrode material is suitable for industrial production and improves the electrochemical performance and structural stability of the material.
Patent Information
- Application Number
- CN202411050047.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing polymetallic composite phosphoric acid/sodium ferric pyrophosphate electropositive electrode material synthesis technology needs to pass co-precipitation reaction, resulting in high cost of equipment and reagents and complex processes, which is not suitable for low-cost and simple industrial production needs, and the working voltage of the material and insufficient energy density limits its wider application range.
Using a simplified preparation method, grinding, spray drying and calcining by mixing sodium salt, doping element source, iron source and phosphorus source at a molar ratio of Na:M:Fe:P=4:3x:3-3x , a polymetallic composite sodium phosphate electropositive electrode material of Na4(MxFe1-x)3(PO4)2P2O7 type was prepared, and the conductive properties and structural stability of the material were improved by using polymetallic elements and carbon coating technology.
The preparation of polymetallic composite sodium phosphate electropositive electrode material with high working voltage and high energy density is achieved, which reduces production costs, simplifies the process flow, is suitable for industrial promotion, and improves the electrochemical performance and structural uniformity of the material.
Smart Images

Figure CN118983437A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a multi-metal element composite sodium phosphate positive electrode material and a preparation method thereof. Background Art
[0002] Due to the consumption of non-renewable energy and environmental pollution, lithium-ion batteries are widely used in the fields of power and energy storage due to their advantages such as high operating voltage and high energy density. However, with the surge in market demand in recent years, the consumption cost of lithium resources has increased significantly, and it is urgent to develop supplementary batteries that can replace lithium-ion batteries in some usage scenarios. Sodium-ion batteries have application prospects in the fields of energy storage and low-speed electric vehicles due to their abundant resources and low cost.
[0003] Among sodium cathode materials, polyanionic compounds have more stable structures and cycle stability than layered transition metal oxides and Prussian blue analogs, and are more in line with the application requirements in the energy storage field. Among them, iron-based composite phosphate Na4Fe3(PO4)2P2O7 (NFPP, theoretical specific capacity 129mAh / g) is regarded as an ideal sodium cathode material for energy storage due to its low cost and high stability. However, its shortcomings of low operating voltage and low energy density limit its application in a wider range, and many practitioners have also focused their research on this.
[0004] CN116504940A discloses a polyanion type sodium ion battery positive electrode material and its preparation method and application. The patented method adopts a co-precipitation combined with high-temperature solid phase sintering method for preparation, wherein the synthesis steps are as follows: a soluble manganese salt, an iron salt and a doping element M source are dissolved in water in a suitable proportion to prepare a mixed solution, the mixed solution, a precipitant and a regulator are added to a reactor protected by an inert atmosphere under the condition of water bath heating, a co-precipitation reaction occurs under rapid stirring to obtain a metal element co-precipitation product, and then the final product is obtained by mechanical mixing, calcination and pulverization.
[0005] Existing synthesis technologies for multi-metal composite phosphoric acid / sodium iron pyrophosphate require a co-precipitation reaction between raw materials, which involves the introduction of a large amount of precipitants and regulators. The precursor synthesis route is complex and has high requirements on the cost of equipment and reagents. It is not suitable for the low cost and simple route requirements of modern large-scale chemical production. Summary of the invention
[0006] The purpose of the present invention is to provide a multi-metal element composite sodium phosphate cathode material with high working voltage and energy density. Another purpose of the present invention is to provide a method for preparing a multi-metal element composite sodium phosphate cathode material with simple route, low cost, environmental friendliness and suitable for large-scale industrialization.
[0007] The present invention discloses a multi-metal composite sodium phosphate positive electrode material, the chemical formula of which is: Na4(M x Fe 1-x )3(PO4)2P2O7, wherein M is one or more of manganese, cobalt, and nickel, and 0.1≤x≤0.9; the average operating voltage is greater than 3.2V.
[0008] Furthermore, the chemical formula of the material is: Na4(M x Fe 1-x )3(PO4)2P2O7, where M is manganese element, 0.25≤x≤0.75.
[0009] If x is greater than 0.75, the Jahn-Teller effect caused by the manganese trivalent ions generated during multiple charge and discharge processes will cause a phase change in the structure of the positive electrode material. In addition, some manganese ions will dissolve in the electrolyte during the cycle, resulting in poor cycle performance of the positive electrode material.
[0010] The present invention also discloses a method for preparing a multi-metal element composite sodium phosphate positive electrode material, comprising the following steps:
[0011] S1. Add sodium salt, doping element M source, iron source, phosphorus source, and solvent and disperse them uniformly according to the molar ratio of Na:M:Fe:P=4:3x:3-3x:4 to form a mixed solution;
[0012] S2, grinding the mixed solution;
[0013] S3, spray drying the ground mixed solution to obtain a precursor;
[0014] S4. Calcinate the precursor to obtain the multi-metal composite sodium phosphate cathode material as described above.
[0015] The sodium source is selected from one or more of sodium dihydrogen phosphate, sodium phosphate, sodium carbonate, sodium citrate, sodium pyrophosphate, disodium dihydrogen pyrophosphate, and sodium acetate; the iron source is selected from one or more of ferric phosphate, ferric nitrate, ferrous oxide, ferrous oxalate, and ferric oxalate; the phosphorus source is selected from one or more of phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium pyrophosphate, and pyrophosphoric acid; the manganese source in the multi-metal source is one or more of manganese nitrate, manganese sulfate, manganese oxalate, and manganese oxide; the cobalt source in the doping element is one or more of cobalt nitrate, cobalt sulfate, cobalt oxalate, and cobalt oxide; the nickel source in the doping element is one or more of nickel nitrate, nickel sulfate, nickel oxalate, and nickel oxide.
[0016] The raw materials used in the preparation method disclosed in the present invention are relatively cheap and widely distributed; and the sand milling, spray drying and calcination processes with low cost, simple route, safety and environmental protection are adopted, which are fully compatible with the current mature lithium iron phosphate material production line and are very easy to promote industrialization.
[0017] Compared with the current co-precipitation process that requires the use of a large amount of precipitants and regulators and has a complicated process, the technical solution of the present invention is a method with a simple route, low cost, environmental friendliness and extremely easy industrialization, and will not introduce additional impurities; in addition, the technical solution prepares a multi-metal element composite sodium phosphate cathode material with uniform particles, high working voltage and good electrochemical performance through the method of multi-metal element composite and carbon coating.
[0018] Furthermore, in the step S1, a carbon source is also added, and the molar ratio of the carbon source to the phosphorus source is 1-10:1.
[0019] The multi-metal element composite sodium phosphate positive electrode material prepared by the present invention has a carbon coating layer, which improves the conductivity of the positive electrode material. The final positive electrode material has the characteristics of good morphology and structure, uniform particles, good electrochemical performance, etc.
[0020] The carbon source is selected from one or more of glucose, sucrose, citric acid, graphite, carbon nanotubes, and graphene.
[0021] Furthermore, in step S1, the solvent is selected from water or ethanol.
[0022] Furthermore, in the step S2, after the mixed solution is ground, the particle size of the particles in the mixed solution is 0.1-1 μm.
[0023] Furthermore, in step S2, the grinding process is performed using a sand mill; the sanding medium used by the sand mill is selected from one or more of zirconium beads and agate beads; the rotation speed of the sand mill is 1000-3000r / min; and the processing time is 1-6h.
[0024] Sanding methods include disc, pin or turbine.
[0025] Furthermore, in step S3, the inlet air temperature of the spray drying is 190-300°C; and the outlet air temperature is 85-120°C.
[0026] Furthermore, in the step S4, the precursor is calcined in an inert gas atmosphere.
[0027] Furthermore, in step S4, the calcination temperature is 450-600° C., the heating rate is 1-5° C. / min, and the constant temperature calcination treatment time is 5-15 h.
[0028] The present invention provides a multi-metal composite sodium phosphate cathode material. The redox potential of iron in the iron-based composite sodium phosphate cathode material is about 3.0V. Therefore, part of the iron in the polyanion structure is replaced by transition metal elements such as manganese, cobalt, and nickel with a higher redox potential (about 3.7V) to obtain a multi-metal composite sodium phosphate cathode material Na4 (M x Fe 1-x )3(PO4)2P2O7. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The Na4(Mn 0.7 Fe 0.3 )3(PO4)2P2O7 SEM image;
[0030] Figure 2 The Na4(Mn 0.7 Fe 0.3 )3(PO4)2P2O7’s XRD pattern. DETAILED DESCRIPTION
[0031] The following will describe the implementation methods of the present application in detail with the accompanying drawings and examples, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly. Based on the examples in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0032] The reagents, methods and equipment used in this application are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in this application are commercially available.
[0033] Example 1
[0034] Preparation of multi-metal composite sodium phosphate cathode material Na4(Mn 0.7 Fe 0.3 )3(PO4)2P2O7:
[0035] Step 1: Take 0.01mol Na4P2O7·10H2O, 0.021mol MnC2O4, 0.009mol Fe(NO3)3·9H2O, 0.02mol NH4H2PO4, and 0.04mol glucose, use ethanol as dispersant, and ball mill for 2h at a speed of 30rpm;
[0036] Step 2: The mixed solution was sand-milled at a speed of 2000 rpm for 3 hours, and the grinding medium was zirconium beads. The particle size of the particles in the mixed solution after grinding was 0.3 μm;
[0037] Step 3: spray-dry the sand-grinding liquid, with an inlet air temperature of 200°C and an outlet air temperature of 110°C to obtain a precursor;
[0038] Step 4: calcine the precursor in an argon atmosphere at a heating rate of 2°C / min and calcine at a constant temperature of 500°C for 15h to obtain the composite phosphoric acid / pyrophosphate manganese iron sodium cathode material Na4(Mn 0.7 Fe 0.3 )3(PO4)2P2O7.
[0039] The obtained composite phosphoric acid / sodium manganese iron pyrophosphate positive electrode material was analyzed by scanning electron microscopy (SEM) and X-ray diffraction analysis (XRD).
[0040] SEM results are as follows Figure 1 As shown, the positive electrode material Na4(Mn 0.7 Fe 0.3 The particles of )3(PO4)2P2O7 are relatively uniform, and the primary particle size is between 100nm and 300nm.
[0041] XRD results are as follows Figure 2 As shown, the positive electrode material Na4(Mn 0.7 Fe 0.3 )3(PO4)2P2O7 is basically consistent with the standard spectrum of iron-based composite phosphate Na4Fe3(PO4)2P2O7 (PDF#89-0579) and has a good peak shape, indicating that the replacement of Fe by Mn in the material does not change the crystal structure of the composite phosphoric acid / sodium iron pyrophosphate material.
[0042] Example 2
[0043] Preparation of multi-metal composite sodium phosphate cathode material Na4(Co 0.3 Fe 0.7 )3(PO4)2P2O7:
[0044] Step 1: Take 0.01mol Na4P2O7·10H2O, 0.09mol CoC2O4, 0.021mol Fe(NO3)3·9H2O, 0.02mol NH4H2PO4, and 0.04mol glucose, use ethanol as dispersant, and ball mill for 2h at a speed of 30rpm;
[0045] Step 2: The mixed solution was passed through a sand mill at a speed of 2200 rpm for 3.5 hours. The grinding medium was zirconium beads. The particle size of the particles in the mixed solution after grinding was 0.3 μm.
[0046] Step 3: spray-dry the sand-grinding liquid, with an inlet air temperature of 200°C and an outlet air temperature of 110°C to obtain a precursor;
[0047] Step 4: calcine the precursor in an argon atmosphere at a heating rate of 2°C / min and calcine at a constant temperature of 480°C for 15h to obtain the composite phosphoric acid / pyrophosphate cobalt iron sodium cathode material Na4(Co 0.3 Fe 0.7 )3(PO4)2P2O7.
[0048] Example 3
[0049] Preparation of non-carbon-coated multi-metal composite sodium phosphate cathode material Na4(Co 0.3 Fe 0.7 )3(PO4)2P2O7:
[0050] Step 1: Take 0.01mol Na4P2O7·10H2O, 0.09mol CoC2O4, 0.021mol Fe(NO3)3·9H2O, and 0.02mol NH4H2PO4, use ethanol as dispersant, and ball mill for 2h at a speed of 30rpm;
[0051] Step 2: The mixed solution was passed through a sand mill at a speed of 2200 rpm for 3.5 hours. The grinding medium was zirconium beads. The particle size of the particles in the mixed solution after grinding was 0.3 μm.
[0052] Step 3: spray-dry the sand-grinding liquid, with an inlet air temperature of 200°C and an outlet air temperature of 110°C to obtain a precursor;
[0053] Step 4: calcine the precursor in an argon atmosphere at a heating rate of 2°C / min and calcine at a constant temperature of 480°C for 15h to obtain a composite phosphoric acid / pyrophosphate cobalt iron sodium positive electrode material Na4(Co 0.3 Fe 0.7 )3(PO4)2P2O7.
[0054] Example 4
[0055] Preparation of multi-metal composite sodium phosphate cathode material Na4(Mn 0.8 Fe 0.2 )3(PO4)2P2O7:
[0056] Step 1: Take 0.01mol Na4P2O7·10H2O, 0.024mol MnC2O4, 0.006mol Fe(NO3)3·9H2O, and 0.02mol NH4H2PO4, use ethanol as dispersant, and ball mill for 2h at a speed of 30rpm;
[0057] Step 2: The mixed solution was sand-milled at a speed of 2000 rpm for 3 hours, and the grinding medium was zirconium beads. The particle size of the particles in the mixed solution after grinding was 0.3 μm;
[0058] Step 3: spray-dry the sand-grinding liquid, with an inlet air temperature of 200°C and an outlet air temperature of 110°C to obtain a precursor;
[0059] Step 4: calcine the precursor in an argon atmosphere at a heating rate of 2°C / min and calcine at a constant temperature of 500°C for 15h to obtain the composite phosphoric acid / pyrophosphate manganese iron sodium cathode material Na4(Mn 0.8 Fe 0.2 )3(PO4)2P2O7.
[0060] Comparative Example 1
[0061] Iron-based composite phosphoric acid / sodium iron pyrophosphate Na4Fe3(PO4)2P2O7, the preparation method of the material is:
[0062] Step 1: Take 0.01 mol Na4P2O7·10H2O, 0.06 mol FePO4, 0.04 mol CH3COONa, and 0.04 mol citric acid monohydrate, use ethanol as dispersant, and ball mill for 2 h at a speed of 30 rpm;
[0063] Step 2: Sand grind the dispersed solution at 2000 rpm for 4 hours, using zirconium beads as the grinding medium and a grinding particle size of 0.3 μm;
[0064] Step 3: spray-dry the sand-grinding liquid, with an inlet air temperature of 200°C and an outlet air temperature of 110°C to obtain a precursor;
[0065] Step 4: Calcine the precursor, place it in an argon atmosphere, and calcine it at a constant temperature of 450°C for 15 hours with a heating rate of 3°C / min to obtain the iron-based composite sodium phosphate cathode material Na4Fe3(PO4)2P2O7.
[0066] Electrochemical performance test:
[0067] The sodium battery positive electrode materials obtained in Examples 1-4 and Comparative Example 1 were processed into positive electrode sheets, which were then assembled into 2032 button cells to test the electrical properties of the sodium battery positive electrode materials.
[0068] The assembly and performance test method of the button cell is as follows: the positive electrode active material (sodium positive electrode material prepared in the example or comparative example), the conductive agent and PVDF are mixed in a mass ratio of 90:5:5, NMP is used as a solvent, and the mixture is evenly coated on an aluminum foil after being stirred and homogenized, and dried overnight in a vacuum oven at 100°C, and then rolled after drying. The diameter of the electrode is 13 mm; a 2032 button cell is assembled in a vacuum glove box, wherein the cell uses a metal sodium sheet as the negative electrode, a glass fiber as the separator, and an electrolyte component of 1 mol L -1 The NaClO4 was dissolved in EC / PC (1:1vt%) solvent and 5vt% FEC was added as an additive; the assembled button cell was tested for its initial charge and discharge capacity at a voltage range of 1.5-4.0V and a rate of 0.1C, and the working average voltage of the battery was derived. The 1C rate discharge capacity was further tested and the capacity retention rate of the material was calculated after the battery was cycled 100 times at 1C. The test results are shown in Table 1 below.
[0069] Table 1 Electrical performance test results
[0070]
[0071] Example 1 Product Na4(Mn 0.7 Fe 0.3 )3(PO4)2P2O7 and the product of Example 2 Na4(Co 0.3 Fe 0.7 )3(PO4)2P2O70.1C first cycle discharge capacity are 105.7mAh / g and 100.9mAh / g respectively, 1C discharge capacity are 101.3mAh / g and 99.6mAh / g respectively, the average working voltage is 3.41V and 3.29V respectively, the capacity retention rate after 100 cycles at 1C is 99.3% and 99.4% respectively. Compared with the iron-based composite phosphoric acid / sodium iron pyrophosphate Na4Fe3(PO4)2P2O7 in Comparative Example 1, it has higher working voltage (3.08V) and electrochemical performance (0.1C discharge 93.9mAh / g, 1C discharge 90.7mAh / g), and the appropriate multi-metal composite amount does not affect the intrinsic cycle performance of the material.
[0072] Example 3 Product Na4(Co 0.3 Fe 0.7 Since )3(PO4)2P2O7 is not carbon-coated, the material has poor conductivity and exhibits poor electrochemical performance. The 0.1C first cycle discharge capacity and 1C discharge capacity are only 91.8mAh / g and 85.0mAh / g respectively, and the capacity retention rate after 100 cycles at 1C is only 94.1%.
[0073] Example 4 Product Na4(Mn 0.8 Fe0.2 The 0.1C first cycle discharge capacity and 1C discharge capacity of )3(PO4)2P2O7 are 106.0mAh / g and 102.2mAh / g respectively, and the average discharge working voltage reaches 3.45V, which performs well. However, due to the excessive manganese content (x>0.75), Mn 3+ The Jahn Teller effect will cause a phase change in the material structure. In addition, some manganese ions will dissolve in the electrolyte during the cycle, causing the material's cycle performance to deteriorate. The measured capacity retention rate after 100 cycles at 1C is only 83.0%, which proves the above point of view.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A multi-metal composite sodium phosphate positive electrode material, characterized in that: The chemical formula of this material is: Na4(M x Fe 1-x )3(PO4)2P2O7, wherein M is one or more of manganese, cobalt, and nickel, and 0.1≤x≤0.9; the average operating voltage is greater than 3.2V.
2. The multi-metal composite sodium phosphate positive electrode material according to claim 1, characterized in that: The chemical formula of this material is: Na4(M x Fe 1-x )3(PO4)2P2O7, where M is manganese element, 0.25≤x≤0.
75.
3. A method for preparing a multi-metal element composite sodium phosphate positive electrode material, characterized in that: The following steps are involved: S1. Add sodium salt, doping element M source, iron source, phosphorus source, and solvent and disperse them uniformly according to the molar ratio of Na:M:Fe:P=4:3x:3-3x:4 to form a mixed solution; S2, grinding the mixed solution; S3, spray drying the ground mixed solution to obtain a precursor; S4. Calcinate the precursor to obtain the multi-metal composite sodium phosphate cathode material as described in any one of claims 1-2.
4. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 3, characterized in that: In the step S1, a carbon source is also added, and the molar ratio of the carbon source to the phosphorus source is 1-10:
1.
5. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 3, characterized in that: In the step S1, the solvent is selected from water or ethanol.
6. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 3, characterized in that: In the step S2, after the mixed solution is ground, the particle size of the particles in the mixed solution is 0.1-1 μm.
7. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 6, characterized in that: In step S2, the grinding process is performed using a sand mill; the grinding medium used by the sand mill is selected from one or more of zirconium beads and agate beads; the rotation speed of the sand mill is 1000-3000r / min; and the processing time is 1-6h.
8. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 3, characterized in that: In step S3, the inlet air temperature of the spray drying is 190-300°C; the outlet air temperature is 85-120°C.
9. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 3, characterized in that: In the step S4, the precursor is calcined in an inert gas atmosphere.
10. The method for preparing a multi-metal composite sodium phosphate positive electrode material according to claim 9, characterized in that: In the step S4, the calcination temperature is 450-600° C., the heating rate is 1-5° C. / min, and the constant temperature calcination treatment time is 5-15 hours.
Citation Information
Patent Citations
Polyanionic sodium-ion battery positive electrode material as well as preparation method and application thereof
CN116504940A