Conductive slurry additive for solid-state or semi-solid-state lithium battery and application and product thereof
By using the composite conductive paste additive of MXeneTi3C2 and carbon nanotubes in solid or semi-solid lithium batteries, the problems of solvent residue, insufficient dispersion and high cost during the preparation of carbon nanotube conductive paste are solved, and the battery efficiency and Stability, achieving more efficient battery performance.
Patent Information
- Application Number
- CN202411064970.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
There are problems of solvent residue, insufficient dispersion and stability, and high cost in the preparation process of existing solid or semi-solid lithium batteries, which limit its large-scale application in batteries.
The complex cooperation between MXeneTi3C2 and carbon nanotubes is used as a conductive paste additive to form a stable dispersion through surface modification and ultrasonic treatment, which improves conductivity and mechanical stability, reduces solution concentration, and introduces a variety of functions to improve interface contact effect through modification. .
It significantly improves the battery efficiency, circulation performance and battery attenuation of solid or semi-solid lithium batteries, reduces costs, and improves conductivity and interface stability.
Smart Images

Figure BDA0004979075680000111 
Figure BDA0004979075680000121
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of batteries and relates to a solid-state or semi-solid-state lithium battery, and in particular to a conductive slurry additive for a solid-state or semi-solid-state lithium battery and an application and product thereof. Background Art
[0002] Solid-state or semi-solid-state batteries refer to batteries that use solid or gel-like electrolytes instead of traditional liquid electrolytes. They have the advantages of higher safety, energy density, and cycle life, and have good technical prospects.
[0003] Solid-state batteries use solid electrolytes, eliminating the flammable and explosive drawbacks of liquid electrolyte lithium batteries, greatly improving battery safety. Semi-solid-state batteries use electrode slurry as the main body of the electrochemical reaction, dispersing active material particles that can deintercalate lithium and conductive agent particles in the electrolyte to form an electrochemical energy storage technology for electrode materials.
[0004] At present, there are three main technical routes for solid-state or semi-solid-state batteries: polymer solid-state batteries, sulfide solid-state batteries and oxide solid-state batteries. Among them, polymer solid-state batteries are the earliest industrialized technical route, but the low ion conductivity at low temperatures limits its application range; sulfide solid-state batteries have the highest room temperature conductivity, but the interface stability between the electrolyte and the electrode material is poor and prone to oxidation reactions; oxide solid-state batteries have high electrochemical stability and cycle performance, but the interface contact between the electrolyte and the electrode material is poor, resulting in high interface impedance.
[0005] Since all-solid-state batteries still have many technical difficulties that need to be overcome, semi-solid-state batteries have taken the lead in entering the mass production stage by reducing the liquid electrolyte content and increasing the solid electrolyte coating, combining safety, energy density and economy. At present, many companies at home and abroad are committed to the technical development and application of semi-solid-state batteries.
[0006] Carbon nanotube conductive slurry is a uniformly dispersed liquid material composed of carbon nanotubes, solvents and dispersants. It has the advantages of high conductivity, high specific surface area and high strength. It can be used as a conductive agent for solid-state batteries to improve the performance and safety of solid-state batteries.
[0007] The application of carbon nanotube conductive paste in solid-state batteries mainly includes: as a conductive additive for positive and negative electrodes, it enhances the conductivity and structural stability of the electrodes, reduces the internal resistance and polarization of the electrodes, and improves the capacity and power of the electrodes; as a conductive additive for solid electrolytes, it improves the conductivity and ion transmission number of solid electrolytes, reduces the internal resistance and interface impedance of solid electrolytes, and improves the electrochemical stability and cycle performance of solid electrolytes; as a connector between positive and negative electrodes and solid electrolytes, it promotes the interface contact and bonding between positive and negative electrodes and solid electrolytes, reduces interface impedance and interface reaction, and improves the charge transfer efficiency and interface stability of the interface.
[0008] The application of carbon nanotube conductive paste in solid-state batteries has the following disadvantages:
[0009] (1) In the preparation process of carbon nanotube conductive slurry, organic solvents and dispersants are required. These substances may have adverse effects on the materials and performance of solid-state batteries, such as solvent residues, dispersant adsorption, and electrochemical instability.
[0010] (2) The dispersion and stability of carbon nanotube conductive slurry need to be further improved. Carbon nanotubes are prone to agglomeration and sedimentation, which affects the uniformity and reliability of the slurry. Some physical or chemical methods are needed to improve the dispersion and stability of carbon nanotubes.
[0011] (3) The cost and price of carbon nanotube conductive paste are relatively high, which limits its large-scale application in solid-state batteries. It is necessary to adopt some low-cost and high-efficiency methods to prepare carbon nanotube conductive paste and reduce its use cost in solid-state batteries.
[0012] The invention patent with publication number CN116779868A discloses a composite conductive agent and silicon-based negative electrode material, silicon-based negative electrode slurry and lithium-ion battery containing the composite conductive agent, wherein the composite conductive agent includes carbon black, carbon nanotubes and sulfonated MXeneTi2C. By compounding carbon black, carbon nanotubes and sulfonated MXene and applying them to negative electrode materials, the conductivity and liquid retention capacity of negative electrode materials can be greatly improved at a low addition amount. It can also effectively prevent the phenomenon of battery performance attenuation caused by the loss of electrical contact of silicon-based negative electrode materials due to expansion, contraction or rupture of silicon particles during the cycle, thereby obtaining a lithium-ion battery with both excellent cycle performance and rate performance.
[0013] The invention patent with publication number CN113611844A discloses a silicon-carbon composite material, a preparation method and application thereof. A graphene foam with carbon nanotubes growing on the surface and in-situ toughened by a carbon nano toughening agent is prepared by chemical vapor deposition, and then Si powder or SiOx powder with carbon nanotubes or carbon nanosheets growing on the surface is loaded into the graphene foam to prepare a flexible electrode based on a silicon-carbon composite material with a novel structure, which can be used as the negative electrode of a semi-solid, quasi-solid or all-solid-state battery, thereby improving the battery's service life, energy density and power density.
[0014] The invention patent with publication number CN113793977B discloses a solid electrolyte and an all-solid-state lithium-ion battery. The solid electrolyte includes inorganic oxygen / sulfide ceramic powder, high molecular polymer and lithium salt. The all-solid-state battery is assembled in situ by using a layer-by-layer coating process, and the polymer diaphragm material is completely replaced by a solid electrolyte. The internal resistance of the battery is reduced by using an in-situ assembly method, and the solid electrolyte is used as an intermediate to improve the safety characteristics of the battery. Graphene film and carbon nanotube film are used as current collector materials to achieve flexible operations such as folding and bending.
[0015] None of the above technologies discloses the application of MXeneTi3C2 and carbon nanotubes in solid-state or semi-solid-state lithium batteries. In view of the above shortcomings, in order to improve the battery efficiency and stability performance of solid-state or semi-solid-state batteries, further improvement of the technology is needed. Summary of the invention
[0016] The present invention aims at the problems existing in the prior art and provides a conductive slurry additive for solid-state or semi-solid-state lithium batteries and its application and product. The present invention adopts MXeneTi3C2 and carbon nanotubes as conductive slurry additives, which are applied to solid-state or semi-solid-state lithium battery electrode slurry, solid-state or semi-solid-state lithium battery electrodes, and solid-state or semi-solid-state lithium batteries, and can improve the battery efficiency, cycle performance and battery attenuation phenomenon of solid-state or semi-solid-state lithium batteries.
[0017] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0018] In a first aspect, the present invention provides a conductive slurry additive for a solid-state or semi-solid-state lithium battery, wherein the conductive slurry additive comprises MXeneTi3C2 and carbon nanotubes, wherein the MXeneTi3C2 is modified MXeneTi3C2 and / or unmodified MXeneTi3C2, and the modification is fluorination modification.
[0019] In the conductive slurry additive for the solid-state or semi-solid-state lithium battery, the carbon nanotubes are selected from one or both of single-walled carbon nanotubes and multi-walled carbon nanotubes. The single-walled carbon nanotubes and multi-walled carbon nanotubes can be selected from commercially available products or can be commercially available products that have been purified. Preferably, the purification is performed by reflux treatment with concentrated nitric acid.
[0020] In the conductive slurry additive of the solid-state or semi-solid-state lithium battery, MXeneTi3C2 can be selected from commercially available products, or MXene Ti3C2 can be obtained by etching its precursor MAX phase.
[0021] In one embodiment, the specific method for preparing the MXene Ti3C2 is: etching the precursor Ti3AlC2 with HF, washing the reaction solution to neutrality (pH ~ 6) after etching, and vacuum drying to obtain MXene Ti3C2. The Ti3AlC2 can be nanometer-scale particle size or micrometer-scale particle size; in one embodiment, the average particle size of the Ti3AlC2 is 0.05-38μm, preferably 30-38μm, more preferably 38μm; in one embodiment, the average particle size of the Ti3AlC2 is 100μm. The mesh size of the Ti3AlC2 can be 200-400 meshes, and in one embodiment, the mesh size of the Ti3AlC2 is 400 meshes.
[0022] The mass ratio of the MXene Ti3C2 to the carbon nanotubes is preferably 5-25:1-25, more preferably 5-25:1-20.
[0023] In the conductive slurry additive for the solid-state or semi-solid-state lithium battery, MXene Ti3C2 and carbon nanotubes can be simply mixed, and MXene Ti3C2 can also be used to modify the carbon nanotubes. The modification of carbon nanotubes by MXene Ti3C2 is specifically as follows: MXeneTi3C2 and carbon nanotubes are dispersed in water respectively, ultrasonically treated to obtain MXeneTi3C2 and carbon nanotube dispersions, mixed, continued ultrasonically treated, centrifuged and dried to obtain the conductive slurry additive.
[0024] The conductive slurry additive for solid-state or semi-solid-state lithium batteries provided by the present invention can improve the problems existing in the application of carbon nanotubes by applying MXeneTi3C2 and carbon nanotubes in solid-state or semi-solid-state lithium batteries, and has the following beneficial effects:
[0025] (1) MXeneTi3C2 has metallic conductive properties. For the first time, the two-dimensional layered MXene Ti3C2 was introduced into the conductive slurry system of one-dimensional carbon nanotubes to form a three-dimensional conductive network, which greatly improved the conductivity and reduced the solution concentration.
[0026] (2) The addition of MXeneTi3C2 can enhance the interaction between carbon nanotube particles through surface modification, thereby stabilizing the dispersion state of carbon nanotubes;
[0027] (3) The two-dimensional morphology of MXene Ti3C2 can be evenly coated on the surface of carbon nanotubes and bridge the gaps between the tubes, thereby enhancing the mechanical stability and conductive pathway of the carbon nanotube network;
[0028] (4) Carbon nanotubes and MXeneTi3C2 can play a synergistic role. With the help of the enhancement effect of MXeneTi3C2, a smaller amount of carbon nanotubes can be used to achieve satisfactory conductivity and network formation effects. The surface of MXene Ti3C2 is modified with chemical groups and added to carbon nanotubes, which can produce synergistic coordination with carbon nanotubes, have good interface contact effects, enhance interface bonding, and improve interface stability. Through control and modification, multiple functions are introduced to achieve composite synergy of conductivity, energy storage, thermal insulation, etc., bringing opportunities for multi-faceted modification and application innovation;
[0029] (5) MXeneTi3C2 aqueous solution has Newton viscosity, which is convenient for preparing stable carbon nanotube mixed dispersions and film casting processes.
[0030] In a second aspect, the present invention provides an application of a conductive slurry additive for solid or semi-solid lithium batteries in solid or semi-solid lithium battery electrode slurry, solid or semi-solid lithium battery electrodes, and solid or semi-solid lithium batteries. The synergistic effect of carbon nanotubes and MXene Ti3C2 in the conductive slurry additive can improve the battery efficiency, cycle performance, and battery attenuation of solid or semi-solid lithium batteries.
[0031] In a third aspect, the present invention provides a solid or semi-solid lithium battery electrode slurry, which is composed of the conductive slurry additive, electrode material, adhesive and solvent described in the above technical solution.
[0032] The mass percentage of each component of the solid or semi-solid lithium battery electrode slurry is: 15-80% conductive slurry additive, 10-75% electrode material, 5-10% adhesive and 0-10% solvent.
[0033] In the solid or semi-solid lithium battery electrode slurry, the electrode material can be any material known to those skilled in the art, and is not limited here. Preferably, the electrode material is selected from one or more of LiMnPO4@S, copper, silicon and carbon, and the carbon can be any type, preferably acetylene black and amorphous carbon.
[0034] In the solid or semi-solid lithium battery electrode slurry, the binder can be any material known to those skilled in the art, and is not limited here. Preferably, the binder is selected from one or more of polyethylene oxide, polydimethylsiloxane and polyvinylidene fluoride.
[0035] In the solid or semi-solid lithium battery electrode slurry, the solvent can be any material known to those skilled in the art, and is not limited here. Preferably, the solvent is selected from one or both of the ionic liquid 1-n-butyl-1-methylpyrrole bis(trifluoromethylsulfonyl)imide salt and N-methylpyrrolidone.
[0036] The viscosity of the solid or semi-solid lithium battery electrode slurry is 2500-4000 mPa·s. In one embodiment, the viscosity of the solid or semi-solid lithium battery electrode slurry is 2500-3500 mPa·s. In one embodiment, the viscosity of the solid or semi-solid lithium battery electrode slurry is 3000-4000 mPa·s.
[0037] In one embodiment, the solid or semi-solid lithium battery electrode slurry comprises the following components in percentage by weight: 80% conductive slurry additive, 10% electrode material and 10% binder, wherein the electrode material is preferably acetylene black, and the binder is preferably polyvinylidene fluoride.
[0038] In one embodiment, the solid or semi-solid lithium battery electrode slurry includes the following components in percentage by weight: 65% LiMnPO4@S, 10% polyethylene oxide (PEO), 15% MXene Ti3C2 modified carbon nanotubes and 10% N-butyl-N-methylpyrrole di(trifluoromethylsulfonyl)imide ([Pyr14]TFSI) ionic liquid. The electrode slurry is a S-sulfonated nano-LiMnPO4 positive electrode slurry, and the composite of MXeneTi3C2 and carbon nanotubes forms a supporting skeleton, and the ionic liquid is loaded to construct a three-dimensional conductive ion conduction network.
[0039] In one embodiment, the solid or semi-solid lithium battery electrode slurry includes the following components in percentage by weight: 75% Cu microparticles, 15% conductive slurry additives and 10% polydimethylsiloxane. The conductive slurry additives are composed of fluorinated modified MXeneTi3C2 and single-walled carbon nanotubes in a mass ratio of 5:1. The electrode slurry is a copper foil-based current collector slurry. MXene Ti3C2 can achieve a strong connection between carbon nanotubes and Cu particles, so that the current collector has excellent mechanical and conductive properties.
[0040] In one embodiment, the solid or semi-solid lithium battery electrode slurry includes the following components in percentage by weight: 45% Si microparticles, 35% conductive slurry additives, 20% multi-walled carbon nanotubes, 15% Ti3C2 nanospheres, 10% amorphous carbon and 10% polyvinylidene fluoride. The conductive slurry additive is composed of MXeneTi3C2 powder and multi-walled carbon nanotubes in a mass ratio of 15:20, and the electrode slurry is a Si-C composite positive electrode current collector slurry with stability.
[0041] The solid or semi-solid lithium battery electrode slurry provided by the present invention is prepared as an electrode, and the carbon nanotubes and MXeneTi3C2 can play a synergistic role. At the same time, through the synergistic effect with the active material interface, the stability of the electrode structure and the interface bonding strength are enhanced, the initial capacity and efficiency of the composite electrode are improved, and the rapid electron and ion conduction is beneficial to the charge and discharge reaction rate and kinetic process of the active material.
[0042] In a third aspect, the present invention provides a solid or semi-solid lithium battery electrode, comprising the solid or semi-solid lithium battery electrode slurry described in the above technical solution. The solid or semi-solid lithium battery electrode can be a positive electrode or a negative electrode.
[0043] In one embodiment, a semi-solid lithium battery electrode is a positive electrode, the positive electrode is composed of a current collector and a positive electrode slurry, the current collector is aluminum foil, the positive electrode slurry is composed of a ternary positive electrode material, a semi-solid lithium battery electrode slurry and a binder, the mass ratio of the ternary positive electrode material, the semi-solid lithium battery electrode slurry and the binder is preferably 85-95:2-10:1-5, more preferably 92:6:2, and the ternary positive electrode material is preferably NCM811.
[0044] In one embodiment, a semi-solid lithium battery electrode is a negative electrode, the negative electrode is composed of a current collector and a negative electrode slurry, the current collector is copper foil, the negative electrode slurry is composed of graphite, a semi-solid lithium battery electrode slurry and a binder, and the mass ratio of the graphite, the semi-solid lithium battery electrode slurry and the binder is preferably 85-95:2-10:1-5, more preferably 94:4:2.
[0045] The carbon nanotubes and MXeneTi3C2 in the solid or semi-solid lithium battery electrode obtained by the present invention can synergistically enhance the efficiency, improve the conductivity of the electrode, and improve the battery efficiency.
[0046] In a fourth aspect, the present invention provides a solid or semi-solid lithium battery, comprising the solid or semi-solid lithium battery electrode described in the above technical solution. The application of carbon nanotubes and MXeneTi3C2 in solid or semi-solid lithium batteries can effectively improve battery efficiency, cycle performance and stability, and alleviate battery attenuation.
[0047] The present invention provides a conductive paste additive for a solid or semi-solid lithium battery and its application and product, wherein the conductive paste additive for a solid or semi-solid lithium battery comprises MXeneTi3C2 and carbon nanotubes, wherein the MXeneTi3C2 is a modified MXeneTi3C2 and / or an unmodified MXeneTi3C2, and the modification is a fluorination modification. The carbon nanotubes and MXene Ti3C2 have a synergistic effect and are applied to solid or semi-solid lithium battery electrode slurry, solid or semi-solid lithium battery electrode, and solid or semi-solid lithium battery, and can improve the battery efficiency, cycle performance and battery attenuation phenomenon of the solid or semi-solid lithium battery. DETAILED DESCRIPTION
[0048] It is worth noting that, unless otherwise specified, the raw materials used in the present invention are all common commercially available products, and their sources are not specifically limited.
[0049] The following sources of raw materials are provided for illustrative purposes:
[0050] Ti3AlC2 powder: purchased from Suzhou Beike Nanotechnology Co., Ltd., purity >98%, average particle size 38μm, 400 mesh.
[0051] N-Methylpyrrolidone (NMP): analytical grade;
[0052] Acetylene black (AB): average particle size 40nm;
[0053] Polyvinylidene fluoride (PVDF): molecular weight is about 500,000.
[0054] Basic Example 1: Preparation of a conductive slurry additive consisting of MXeneTi3C2 powder and multi-walled carbon nanotubes
[0055] Preparation of MXeneTi3C2 powder: HF etching method was used to prepare it. 10g Ti3AlC2 powder was added to 40% HF solution (100mL), stirred and etched for 2 hours. Then it was washed with deionized water until neutral, centrifuged (3500rpm, 10min), and vacuum dried at 60℃ for 12 hours to obtain MXeneTi3C2 powder.
[0056] Preparation of multi-walled carbon nanotube (CNT) powder: Multi-walled carbon nanotubes (purity>95%, diameter 10-20nm, length 10-30μm) were refluxed in concentrated nitric acid for 6 hours to remove impurities, washed with deionized water to neutrality, and vacuum dried at 60°C for 12 hours to obtain carbon nanotube powder.
[0057] 5.0 g of MXeneTi3C2 powder and 1.0 g of multi-walled carbon nanotube powder were simply mixed to obtain a conductive slurry additive.
[0058] Basic Example 2: Preparation of a conductive paste additive composed of MXeneTi3C2 modified carbon nanotubes
[0059] MXeneTi3C2 modified carbon nanotubes: 0.1g MXeneTi3C2 powder (prepared in basic example 1) was dispersed in 50mL deionized water, ultrasonically treated for 1 hour, 0.01g pretreated CNTs (multi-walled carbon nanotube powder prepared in basic example 1) was dispersed in 50mL deionized water, ultrasonically treated for 1 hour, the two dispersions were mixed, and ultrasonic treatment was continued for 2 hours, stirring speed: 500rpm, temperature: room temperature (25°C), centrifugal separation (5000rpm, 10 minutes), washed with deionized water 3 times. Freeze drying for 24 hours to obtain a conductive slurry additive.
[0060] Basic Example 3: Preparation of a conductive paste additive consisting of fluorinated MXeneTi3C2 and single-walled carbon nanotubes
[0061] Preparation of fluorinated MXeneTi3C2: 50 mL of MXeneTi3C2 powder (prepared in Basic Example 1) dispersion (MXeneTi3C2 concentration is 2 mg / mL) was mixed with 5 mL of NH4HF2 solution (NH4HF2 concentration is 40 mg / mL), stirred at 25°C, and reacted at a speed of 300 rpm. The mixture was reacted for 24 hours, centrifuged (5000 rpm, 10 minutes), washed with deionized water and ethanol three times, and vacuum dried at 60°C for 12 hours.
[0062] Single-walled carbon nanotubes (CNTs): purchased from Xianfeng Nanotechnology Co., Ltd., with a purity of >95%, a diameter of 1-2nm, and a length of 5-30μm.
[0063] 5 g of MXeneTi3C2 modified with fluorinated groups and 10 g of single-walled carbon nanotubes were simply mixed in a mass ratio of 5:10 to obtain a conductive slurry additive.
[0064] Basic Example 4: Preparation of a conductive paste additive consisting of ultra-small MXene Ti3C2 powder (average particle size of 100 nm) and multi-walled carbon nanotubes
[0065] Preparation of ultra-small MXeneTi3C2 powder: Ti3AlC2 MAX phase was ball-milled to 100nm using high-energy ball milling to obtain Ti3AlC2 powder, and then HF etching was used to add 10g Ti3AlC2 powder to 40% HF solution (100mL), and stirred and etched for 2 hours. After that, it was washed with deionized water until neutral, centrifuged (3500rpm, 10min), and vacuum dried at 60℃ for 12 hours to obtain ultra-small MXene Ti3C2 powder.
[0066] The ultra-small MXeneTi3C2 powder and the multi-walled carbon nanotube powder (prepared in Basic Example 1) were simply mixed in a mass ratio of 15:20 to obtain a conductive slurry additive.
[0067] Example 1: Preparation of electrode slurry
[0068] Electrode material: acetylene black.
[0069] Electrolyte: Polyvinylidene fluoride is selected.
[0070] Solvent: N-methylpyrrolidone is selected.
[0071] 4 g of the conductive paste additive prepared in Basic Example 1 was added to a ball mill, and 25 mL of N-methylpyrrolidone was added. The mixture was wet-milled at 300 rpm for 4 hours, and the milling was stopped for 5 minutes every hour to avoid overheating. 0.5 g of acetylene black and 0.5 g of polyvinylidene fluoride were weighed, added to the ball mill, and the milling was continued at 300 rpm for 2 hours. The milled slurry was transferred to a vacuum agitator, stirred at a vacuum degree of 0.1 MPa for 45 minutes at a speed of 500 rpm, and the bubbles in the slurry were removed to obtain an electrode slurry with a viscosity of 3632 mPa·s.
[0072] Example 2: Preparation of electrode slurry
[0073] 1.5g of the conductive paste additive (15wt%) prepared in Basic Example 2 was added to a ball mill, and 6.5g of LiMnPO4@S (65wt%), 1g of polyethylene oxide (PEO, 10wt%) and 1g of N-butyl-N-methylpyrrole di(trifluoromethylsulfonyl)imide salt ([Pyr14]TFSI, 10wt%) were weighed and added to the ball mill, and ball milled at 300rpm for 2 hours. The ball-milled slurry was transferred to a vacuum agitator and stirred at a vacuum degree of 0.1MPa for 45 minutes at a speed of 500rpm to remove bubbles in the slurry to obtain an electrode slurry with a viscosity of 3146mPa·s.
[0074] Example 3: Preparation of electrode slurry
[0075] 1.5g of the conductive paste additive (15wt%) prepared in Basic Example 3 was added to a ball mill, and 7.5g of Cu particles (75wt%) and 1g of polydimethylsiloxane (10wt%) were weighed and added to the ball mill, and ball milled at 300rpm for 2 hours. The ball-milled slurry was transferred to a vacuum stirrer and stirred at a vacuum degree of 0.1MPa for 45 minutes at a speed of 500rpm to remove bubbles in the slurry to obtain an electrode slurry with a viscosity of 2575mPa·s.
[0076] Example 4: Preparation of electrode slurry
[0077] 3.5 g of the conductive paste additive (35 wt%) prepared in Basic Example 4 was added to a ball mill, and 4.5 g of Si particles (45 wt%), 1 g of amorphous carbon (10 wt%) and 1 g of polyvinylidene fluoride (PVDF, 10 wt%) were weighed and added to the ball mill, and ball milled at 300 rpm for 2 hours. The ball-milled slurry was transferred to a vacuum agitator and stirred at a vacuum degree of 0.1 MPa for 45 minutes at a speed of 500 rpm to remove bubbles in the slurry to obtain an electrode slurry with a viscosity of 3500 mPa·s.
[0078] Example 5: Preparation of electrode slurry
[0079] The difference from Example 1 is that "4 g of the conductive slurry additive prepared in Basic Example 1" is replaced by "3.33 g of MXene Ti3C2 powder and 0.67 g of multi-walled carbon nanotubes prepared in Basic Example 1", and the other steps and operations are the same as those in Example 1, and an electrode slurry with a viscosity of 3851 mPa·s is obtained.
[0080] Example 6: Preparation of electrode slurry
[0081] The difference from Example 1 is that "4 g of the conductive slurry additive prepared in Basic Example 1" is replaced by "2.67 g of MXene Ti3C2 powder and 1.33 g of multi-walled carbon nanotubes prepared in Basic Example 1", and the other steps and operations are the same as those in Example 1, and an electrode slurry with a viscosity of 3786 mPa·s is obtained.
[0082] Comparative Example 1:
[0083] The difference from Example 1 is that the "conductive slurry additive prepared in Basic Example 1" is replaced by "MXeneTi3C2 powder (prepared in Basic Example 1)", and the other steps and operations are the same as those in Example 1 to obtain an electrode slurry with a viscosity of 4114 mPa·s.
[0084] Comparative Example 2:
[0085] The difference from Application Example 1 is that the "conductive slurry additive prepared in Basic Example 1" is replaced by "multi-walled carbon nanotube powder (prepared in Basic Example 1)", and the other steps and operations are the same as those in Example 1 to obtain an electrode slurry with a viscosity of 3137 mPa·s.
[0086] Comparative Example 3:
[0087] Preparation of MXeneTi2C: The method for preparing MXeneTi3C2 powder in Basic Example 1 is adopted, wherein Ti2AlC is used instead of Ti3AlC2 to prepare MXeneTi2C.
[0088] The difference from Example 1 is that "MXeneTi3C2 powder in the conductive slurry additive prepared in Basic Example 1" is replaced by "MXeneTi2C", and the other steps and operations are the same as those in Example 1, and an electrode slurry with a viscosity of 3817 mPa·s is obtained.
[0089] Comparative Example 4:
[0090] Sulfonated MXeneTi3C2: 1 g of MXene Ti3C2 powder (prepared in Basic Example 1) was reacted with 20 mL of concentrated sulfuric acid at 60° C. for 4 hours, washed and dried to obtain sulfonated MXeneTi3C2.
[0091] The difference from Example 1 is that "MXeneTi3C2 powder in the conductive slurry additive prepared in Basic Example 1" is replaced by "MXeneTi3C2 modified by sulfonation", and the other steps and operations are the same as those in Example 1 to obtain an electrode slurry with a viscosity of 3953 mPa·s.
[0092] Application Example 1:
[0093] Preparation of semi-solid lithium battery:
[0094] (1) Preparation of positive and negative electrodes:
[0095] The positive electrode component ratio is NCM811: the electrode slurry of Example 1: PVDF = 92:6:2 (weight ratio). NCM811 (Shenzhen Grep Battery Co., Ltd.) and PVDF are added to the electrode slurry, stirred and mixed for 4 hours, and ground 3 times using a three-roll grinder to obtain a uniform positive electrode slurry. The slurry is coated on aluminum foil (coating thickness 150μm, aluminum foil thickness 16μm), and vacuum dried at 80℃ for 12 hours. Roll to a positive electrode thickness of 120μm, a porosity of 25-30%, and cut into discs with a diameter of 14mm.
[0096] Negative electrode preparation:
[0097] The positive electrode component ratio is artificial graphite: electrode slurry of Example 1: PVDF = 94:4:2 (weight ratio), and the negative electrode slurry is prepared according to the steps similar to the positive electrode preparation. The slurry is coated on copper foil (coating thickness 130μm, copper foil thickness 8μm), and vacuum dried at 60℃ for 12 hours. The negative electrode is rolled to a thickness of 110μm, a porosity of 30-35%, and cut into discs with a diameter of 15mm.
[0098] (2) Preparation of semi-solid electrolyte:
[0099] The ratio of the semi-solid electrolyte components is PEGDME (Mw = 500): LiTFSI = 78:22 (weight ratio). LiTFSI (bis(trifluoromethane)sulfonyl imide lithium salt) is dissolved in PEGDME (polyethylene glycol dimethyl ether) in an argon glove box and stirred at 60°C for 12 hours. 2wt% of nano-Al2O3 is added as a thickener, stirring is continued for 6 hours, and ultrasonic treatment is used for 30 minutes to ensure uniform dispersion.
[0100] (3) Battery assembly:
[0101] In an argon glove box (water and oxygen content <0.1ppm), place a PE diaphragm (16mm in diameter, 25μm in thickness) on the negative electrode, inject 120μL of semi-solid electrolyte into the diaphragm, and place the positive electrode sheet on the diaphragm to ensure that the electrolyte is fully infiltrated. Use a 2032-type button battery casing for packaging and apply a pressure of 5MPa. For battery packaging: Use a hydraulic press to press the battery components to ensure that the sealing ring is completely sealed to prevent electrolyte leakage. For battery activation: Place the packaged battery in a 45°C constant temperature box and maintain activation at 5MPa pressure for 24 hours. Obtain a semi-solid lithium battery using the electrode slurry of Example 1.
[0102] Application Examples 2-6 and Comparative Examples 1-4
[0103] The "electrode slurry of Example 1" was replaced with "electrode slurries of Examples 2-6 and Comparative Examples 1-4" respectively, and the other steps and operations were the same as those of Application Example 1 to obtain a semi-solid lithium battery. The obtained semi-solid lithium batteries were named Application Examples 2-6 and Comparative Examples 1-4 respectively.
[0104] Test Case
[0105] Performance Test:
[0106] The battery performance of the semi-solid lithium battery of the test application examples 1-6 and the comparative examples 1-4 was tested, and the charge and discharge test was carried out at room temperature, the voltage range was 2.8V-4.3V, constant current charging was carried out to 4.3V at a rate of 0.05C, and then constant voltage charging was carried out until the current dropped to 0.01C, and then constant current discharge was carried out to 2.8V at a rate of 0.05C, and the first coulomb efficiency was tested, and then constant current charge and discharge were carried out at a rate of 0.2C for 100 cycles, and the rate performance (0.1C, 0.2C, 0.5C, 1C, 2C) was tested, and 100 cycle tests (1C rate) were carried out to evaluate the capacity retention rate. The specific capacity and conductivity of the semi-solid lithium battery were determined. The results are shown in Table 1.
[0107] Table 1 Battery performance test of semi-solid lithium battery
[0108]
[0109]
[0110] The specific capacity (mAh / g) indicates the amount of electricity that can be stored per gram of active material in the battery. A higher specific capacity means that the battery can store more energy. The first coulombic efficiency (%) indicates the ratio of the discharge capacity to the charge capacity in the first charge and discharge cycle of the battery. A higher first coulombic efficiency means less irreversible capacity loss. The capacity retention rate (%) after 100 cycles reflects the cycle stability of the battery. A higher retention rate means that the battery can still maintain a higher capacity after multiple charge and discharge cycles. The rate performance (1C / 0.1C, %) indicates the ratio of the discharge capacity at a high rate (1C) to the discharge capacity at a low rate (0.1C). A higher ratio means that the battery has less performance loss during rapid charge and discharge. The conductivity (S / cm) reflects the conductivity of the electrode material, and a higher conductivity helps improve the power performance of the battery.
[0111] The specific capacity, first coulomb efficiency, capacity retention rate after 100 cycles, rate performance and conductivity of the semi-solid lithium battery of application examples 1-6 are significantly better than those of the semi-solid lithium battery of comparative examples 1-4. Among them, the specific capacity of the semi-solid lithium battery of application example 4 is the highest, reaching 707mAh / g; the first coulomb efficiency is 85%; the capacity retention rate after 100 cycles is 95%; the rate performance is the highest, at 90%; and the conductivity is the highest, at 20S / cm. This may be due to its unique material combination (nanostructured ultra-small MXene Ti3C2 and multi-walled carbon nanotubes) providing a larger specific surface area and better electron conduction path, its electrode-electrolyte interface formation process is the most efficient, the electrode structure is stable, it has excellent fast charge and discharge capabilities and an efficient conductive network, and has better battery performance.
[0112] By comparing the performance of the semi-solid lithium batteries of Application Example 1 and Comparative Examples 1-2, it is found that the composite use of MXeneTi3C2 and carbon nanotubes has better specific capacity, initial coulombic efficiency, capacity retention rate after 100 cycles, rate performance and conductivity than the use of MXeneTi3C2 and carbon nanotubes alone. The synergistic effect of MXeneTi3C2 and carbon nanotubes can provide sufficient conductivity and structural stability, thereby improving battery performance.
[0113] By comparing the performance of the semi-solid lithium batteries of Application Example 1 and Comparative Examples 3-4, it was found that the battery specific capacity, first coulombic efficiency, capacity retention rate after 100 cycles, rate performance and conductivity of the battery using MXeneTi3C2 were better than those of MXeneTi2C and sulfonated MXeneTi3C2.
[0114] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A conductive paste additive for solid or semi-solid lithium batteries, characterized in that: The conductive paste additive includes MXeneTi3C2 and carbon nanotubes, the MXeneTi3C2 is modified MXeneTi3C2 and / or unmodified MXeneTi3C2, and the modification is fluorination modification.
2. The conductive paste additive for solid-state or semi-solid-state lithium batteries according to claim 1, characterized in that: The mass ratio of the MXeneTi3C2 and the carbon nanotubes is 5-25:1-25.
3. The conductive paste additive for solid-state or semi-solid-state lithium batteries according to claim 2, characterized in that: The mass ratio of the MXene Ti3C2 to the carbon nanotubes is 5-25:1-20.
4. Use of the conductive slurry additive for solid-state or semi-solid-state lithium batteries according to any one of claims 1 to 3 in solid-state or semi-solid-state lithium battery electrode slurry, solid-state or semi-solid-state lithium battery electrodes, and solid-state or semi-solid-state lithium batteries.
5. A solid or semi-solid lithium battery electrode slurry, characterized in that: The conductive paste comprises the conductive paste additive according to any one of claims 1 to 3, an electrode material, a binder and a solvent.
6. The solid or semi-solid lithium battery electrode slurry according to claim 5, characterized in that: The mass percentage of each component in the electrode slurry is: 15-80% conductive slurry additive, 10-75% electrode material, 5-10% adhesive and 0-10% solvent.
7. The solid or semi-solid lithium battery electrode slurry according to claim 6, characterized in that: The electrode material is selected from one or more of LiMnPO4@S, copper, silicon and carbon.
8. The solid or semi-solid lithium battery electrode slurry according to claim 6, characterized in that: The adhesive is selected from one or more of polyethylene oxide, polydimethylsiloxane and polyvinylidene fluoride.
9. The solid or semi-solid lithium battery electrode slurry according to claim 6, characterized in that: The solvent is selected from one or both of ionic liquid 1-n-butyl-1-methylpyrrole bis(trifluoromethylsulfonyl)imide salt and N-methylpyrrolidone.
10. The solid or semi-solid lithium battery electrode slurry according to any one of claims 5 to 9, characterized in that: The viscosity of the electrode slurry is 2500-4000 mPa·s.
11. A solid or semi-solid lithium battery electrode, characterized in that: The invention comprises the solid or semi-solid lithium battery electrode slurry as described in any one of claims 5 to 9.
12. A solid or semi-solid lithium battery, characterized in that: Comprising the solid or semi-solid lithium battery electrode as described in claim 11.
Citation Information
Cited By
Composite conductive paste and preparation method thereof, negative electrode material, negative electrode plate and battery