Preparation method of catalytic interlayer material of lithium-sulfur battery and catalytic interlayer material

The porous Ti3C2 MXene fiber membrane is prepared as a functional interlayer for lithium-sulfur batteries through electrospinning technology, which solves the problems of poor conductivity and volume expansion in lithium-sulfur batteries, improves the energy density and cycle stability of the battery, and achieves more efficient electricity. Chemical properties.

CN118983620APending Publication Date: 2024-11-19SOUTHWEAT UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411069453.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing lithium-sulfur battery interlayer materials have poor conductivity, low adsorption strength and volume expansion during the circulation process, resulting in insufficient electrochemical performance and cyclic characteristics, affecting the energy density and stability of lithium-sulfur battery.

Method used

Electrospinning technology was used to introduce Ti3C2 MXene into polyacrylonitrile fibers. By regulating the fiber tube diameter and orientation, porous Ti3C2 MXene fiber membrane was prepared as a functional interlayer, combining physical and chemical adsorption mechanisms to inhibit the polysulfide shuttle effect, and through high temperature Carbonization improves conductivity.

Benefits of technology

It significantly improves the energy density, rate performance and long-term cycle stability of lithium-sulfur batteries, enhances the utilization rate and electrochemical performance of sulfur, and reduces the energy density loss of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983620A_ABST
    Figure CN118983620A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a catalytic interlayer material of a lithium-sulfur battery and the catalytic interlayer material, and belongs to the technical field of lithium-sulfur batteries, and the preparation method comprises the following steps: dispersing multiple layers of Ti3C2TX in water, then carrying out ultrasonic stripping and centrifugation, collecting an upper suspension, and carrying out freeze drying to obtain few layers of Ti3C2MXene; the preparation method comprises the following steps: dissolving polyacrylonitrile in N, N-dimethylformamide, and then adding few layers of Ti3C2MXene to obtain a mixed solution; carrying out electrostatic spinning by taking the mixed solution as a raw material, and then carrying out vacuum drying to obtain a Ti3C2MXene / PAN fiber membrane; the Ti3C2MXene / PAN fiber membrane is subjected to heating pre-oxidation and then subjected to high-temperature carbonization, and the porous Ti3C2MXene fiber membrane is obtained. The catalytic interlayer material prepared by the method can inhibit the shuttle effect of polysulfide in the lithium-sulfur battery, improve the electrochemical performance and cycle characteristics of the lithium-sulfur battery and accelerate the commercialization process of the lithium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium-sulfur batteries, and in particular relates to a preparation method of a catalytic interlayer material for a lithium-sulfur battery and the catalytic interlayer material. Background Art

[0002] With the development of society, people's demand for energy continues to increase. Since traditional fossil energy will inevitably cause environmental pollution, my country clearly proposed the goals of "carbon peak" in 2030 and "carbon neutrality" in 2060 in September 2020, which promoted the vigorous development of clean energy. However, solar energy, wind energy and hydropower are affected by geographical location, environmental climate, etc., and have problems such as instability, discontinuity and intermittency. Therefore, how to store clean energy has become an urgent problem to be solved.

[0003] Currently, lithium-ion batteries have been widely used in commercial applications, but they are gradually unable to meet current needs due to the limitation of energy density. Lithium-sulfur batteries are a very promising new battery system due to their higher energy density and low cost of active material sulfur. However, due to the poor conductivity of sulfur and the shuttle effect of intermediate polysulfides, the large-scale application of lithium-sulfur batteries still faces many challenges. 1. Shuttle effect of polysulfides. During the charge and discharge cycle of the battery, the polysulfides in the battery penetrate the diaphragm under the action of the electric field force and concentration gradient, and shuttle between the positive and negative electrodes to produce a shuttle effect. 2. Volume expansion. Due to the difference in density between S and Li2S, the volume of the cathode material changes greatly during the cycle (≈79%), resulting in mechanical stress and strain in the positive electrode material, affecting the structural integrity and cycle stability of the positive electrode material; 3. Insulation of active materials and discharge products. The conductivity of sulfur and discharge products Li2S2 / Li2S is relatively poor. Among them, Li2S2 / Li2S will accumulate on the surface of lithium metal to produce a deposition layer, which delays the diffusion of ions. In response to the various problems existing in lithium-sulfur batteries at this stage, researchers have made a lot of attempts, such as improving the electrolyte, introducing interlayers, improving separators, etc. Among them, constructing a functional interlayer between the separator and the active electrode is considered to be a reliable and simple method.

[0004] The interlayer not only suppresses the severe shuttle effect by limiting the diffusion of polysulfides to the anode, but also ensures the efficient electrocatalytic conversion of polysulfides, thereby improving the utilization of active materials and the overall electrochemical performance. The functional interlayer as a "polysulfide sieve" is able to physically or chemically adsorb intermediate polysulfides (LiPS). This functional interlayer consists of three parts: a polar material that provides a large number of adsorption sites for effective anchoring of polysulfides, a conductive medium that promotes rapid charge transfer during redox processes, and finally a porous structure that allows effective electrolyte penetration and copes with volume expansion during redox reactions, thereby stabilizing sulfur electrochemical reactions. Various polar materials, such as conductive porous carbon, metal sulfides, metal oxides, metal nitrides, metal phosphides, etc., have been studied as positive electrode interlayers to improve the performance of lithium-sulfur batteries.

[0005] The existing problems of lithium-sulfur battery interlayers are as follows: (1) Traditional interlayer materials, such as conductive carbon materials, generally physically adsorb soluble LiPS, resulting in weak adsorption strength and low ion conductivity due to poor electrolyte wettability, which hinders the cycling and conversion reaction kinetics; (2) The use of metal compounds that can chemically adsorb soluble LiPS as functional interlayers has poor conductivity, resulting in low initial discharge capacity and sulfur utilization; (3) In order to achieve the expected performance, the thickness and weight of traditional interlayers are generally large, which also greatly reduces the overall energy density of the battery system.

[0006] MXene is a class of two-dimensional transition metal carbides and nitrides that provide a promising solution to overcome the shortcomings of carbonaceous matrices. First, MXene has a unique 2D structure, excellent mechanical properties, and chemical stability to lithium metal. Second, it has abundant polar surface functional groups that can coordinately anchor polysulfides (LiPS) through redox and Lewis acid-base interactions. Third, MXenes have high electrical conductivity and low Li + The diffusion coefficient improves the bidirectional conversion kinetics of polysulfides, reduces the overpotential in the lithium plating / stripping process, and improves the electrochemical performance of the sulfur cathode. Therefore, it is considered to have good prospects, but because MXene is easy to stack, it reduces the active sites on its surface, and the stacked block MXene even hinders the conductive path. Therefore, the interface and structure control design of MXene is considered to be an effective strategy to solve the above problems currently encountered. Summary of the invention

[0007] In order to solve the problem of insufficient electrochemical performance and cycle characteristics of existing lithium-sulfur batteries, the present invention provides a method for preparing a catalytic interlayer material for a lithium-sulfur battery. The lithium-sulfur battery catalytic interlayer material prepared by the method can inhibit the polysulfide shuttle effect in the lithium-sulfur battery, improve the electrochemical performance and cycle characteristics of the lithium-sulfur battery, and thus accelerate the commercialization process of the lithium-sulfur battery.

[0008] The invention also provides a lithium-sulfur battery catalytic interlayer material.

[0009] The present invention is achieved through the following technical solutions:

[0010] The present invention provides a method for preparing a catalytic interlayer material for a lithium-sulfur battery, the preparation method comprising:

[0011] Multilayer Ti3C2T X After being dispersed in water, ultrasonic exfoliation was performed, followed by centrifugation, the upper suspension was collected and freeze-dried, and the dried product was ground to obtain a few-layer Ti3C2 MXene;

[0012] Dissolving polyacrylonitrile in N,N-dimethylformamide, and then adding the few-layer Ti3C2 MXene to obtain a mixed solution;

[0013] The mixed solution is used as a raw material for electrospinning, and the obtained product is vacuum dried to obtain a Ti3C2 MXene / PAN fiber membrane;

[0014] The Ti3C2 MXene / PAN fiber membrane is pre-oxidized by heating in an air atmosphere, and then carbonized at a high temperature in an argon atmosphere to obtain a porous Ti3C2 MXene fiber membrane.

[0015] Furthermore, the multilayer Ti3C2T X After being dispersed in water, ultrasonic peeling is performed, followed by centrifugation, the upper suspension is collected and freeze-dried, and the dried product is ground to obtain a few-layer Ti3C2 MXene, which specifically includes:

[0016] Multilayer Ti3C2T X Dispersed in water at a concentration of 2 mg / mL, subjected to ultrasonic exfoliation and centrifugation, the upper suspension was collected and freeze-dried, and the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene.

[0017] Furthermore, the multilayer Ti3C2T X Dispersed in water at a concentration of 2 mg / mL, subjected to ultrasonic exfoliation and centrifugation, the upper suspension was collected and freeze-dried, the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene, specifically comprising:

[0018] Multilayer Ti3C2TX Dispersed in water at a concentration of 2 mg / mL, placed in an ice bath at 350 W for ultrasonic exfoliation for 3 h, then centrifuged at 8000 r / min for 20 min, the upper suspension was collected and freeze-dried, the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene.

[0019] Further, the polyacrylonitrile is dissolved in N,N-dimethylformamide, and then the few-layer Ti3C2 MXene is added to obtain a mixed solution, which specifically includes:

[0020] Dissolving polyacrylonitrile in N,N-dimethylformamide, and then adding the few-layer Ti3C2 MXene to obtain a mixed solution;

[0021] Wherein, in the mixed solution, the concentration of polyacrylonitrile is 0.08±0.01 g / mL, and the content of the few-layer Ti3C2 MXene is 25-75wt%.

[0022] Furthermore, the mixed solution is used as a raw material for electrospinning, and the obtained product is vacuum dried to obtain a Ti3C2MXene / PAN fiber membrane, which specifically includes:

[0023] The mixed solution is used as a raw material for electrospinning, and the obtained product is vacuum dried at 60±5° C. for 12±2 h to obtain a Ti3C2 MXene / PAN fiber membrane;

[0024] Wherein, in the electrospinning process, the flow rate of the mixed solution is 0.4-1 mL / h, and the electrospinning voltage is 12-20 kV.

[0025] Furthermore, the Ti3C2 MXene / PAN fiber membrane is pre-oxidized at a high temperature in an air atmosphere, and then carbonized at a high temperature in an argon atmosphere to obtain a porous Ti3C2 MXene fiber membrane, specifically comprising:

[0026] The Ti3C2 MXene / PAN fiber membrane was pre-oxidized by heating the Ti3C2 MXene / PAN fiber membrane to 250±10°C at 2°C / min in an air atmosphere for 1±0.5h, and then carbonized by heating the Ti3C2 MXene / PAN fiber membrane to 700±50°C at 5°C / min in an argon atmosphere for 1±0.2h to obtain a porous Ti3C2 MXene fiber membrane.

[0027] Based on the same inventive concept, the present invention provides a lithium-sulfur battery catalytic interlayer material, and the catalytic interlayer material is prepared by the above-mentioned preparation method of a lithium-sulfur battery catalytic interlayer material.

[0028] Based on the same inventive concept, the present invention provides a lithium-sulfur battery, wherein the lithium-sulfur battery comprises the above-mentioned lithium-sulfur battery catalytic interlayer material.

[0029] Based on the same inventive concept, the present invention provides a method for preparing a lithium-sulfur battery, the preparation method comprising:

[0030] Cutting the above-mentioned lithium-sulfur battery catalytic interlayer material into discs with a diameter of 19 mm to obtain a lithium-sulfur battery interlayer;

[0031] The lithium-sulfur battery interlayer is assembled with the positive electrode shell, the positive electrode, the separator, the lithium sheet, the gasket, the shrapnel and the negative electrode shell to form a lithium-sulfur battery.

[0032] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0033] 1. The present invention discloses a method for preparing a catalytic interlayer material for a lithium-sulfur battery. The method introduces Ti3C2MXene into polyacrylonitrile fibers with adjustable size and orientation through electrostatic spinning technology, and adjusts the diameter and orientation of the polyacrylonitrile fibers to achieve the purpose of regulating the specific surface area and porosity of the Ti3C2MXene fiber membrane. Polyacrylonitrile has the advantages of high carbonization rate and stable structure after carbonization. The porous Ti3C2MXene fiber membrane obtained after carbonization is assembled into a lithium-sulfur battery system as its functional interlayer, which can solve the problems of volume expansion shuttle effect and sulfur non-conductivity occurring during the battery cycle, and finally achieve the purpose of improving the energy density, rate performance and long-term cycle stability of the lithium-sulfur battery.

[0034] 2. The present invention discloses a lithium-sulfur battery catalytic interlayer material. A multifunctional MXene interlayer composed of carbon nanofibers and Ti3C2 MXene with controllable structural morphology is developed through electrospinning technology. The interlayer plays multiple roles in improving the performance of lithium-sulfur batteries. First, the porous Ti3C2 MXene fiber membrane of the present invention is a three-dimensional network structure, which can physically adsorb LiPS. In addition, Ti3C2 MXene coordinates and anchors LiPS (chemical adsorption) through redox and Lewis acid-base interactions. This combination of physical and chemical adsorption can effectively inhibit the shuttling phenomenon and enhance the cycle stability. Secondly, Ti3C2 MXene greatly improves the wettability of the electrolyte due to its greater hydrophilicity, and the large specific surface area of ​​the three-dimensional network structure provides more nucleation sites, thereby increasing the utilization rate of sulfur. The carbon nanofibers obtained through the carbonization process and the conductive Ti3C2 MXene itself can accelerate the cycle and conversion reaction kinetics. Finally, the MXene interlayer manufactured by electrospinning can achieve precise control of mass and thickness over a large area, thereby minimizing the energy density loss of the lithium-sulfur battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0036] Figure 1 Schematic diagram of the preparation process and action mechanism of the catalytic interlayer material for lithium-sulfur batteries of the present invention;

[0037] Figure 2 The SEM images of Ti3C2 MXene / PAN fiber membranes at different Ti3C2 MXene contents in Example 1 of the present invention;

[0038] Figure 3 The SEM images of the porous Ti3C2 MXene fiber membranes with different Ti3C2 MXene contents in Example 1 of the present invention;

[0039] Figure 4 This is a physical picture of the porous Ti3C2 MXene fiber membrane with different Ti3C2 MXene contents in Example 1 of the present invention;

[0040] Figure 5 This is the SEM image of Ti3C2 MXene before and after peeling in Example 2 of the present invention;

[0041] Figure 6 XRD patterns of Ti3C2 MXene before and after exfoliation in Example 2 of the present invention;

[0042] Figure 7 The cyclic performance spectrum of the Ti3C2 MXene fiber membrane with a Ti3C2 MXene content of 50wt% in Example 2 of the present invention applied as a functional interlayer to a lithium-sulfur battery under a high load of 0.2C;

[0043] Figure 8 The cyclic stability performance spectrum of Ti3C2 MXene fiber membranes with different Ti3C2 MXene contents in Example 2 of the present invention applied as functional interlayers in lithium-sulfur batteries at 0.5C;

[0044] Fig. 9 2C cycle stability spectrum of Ti3C2 MXene fiber membrane with 0wt.% and 50wt.% Ti3C2 MXene content in Example 2 of the present invention used as a functional interlayer in a lithium-sulfur battery;

[0045] Fig.10The rate performance spectrum of the Ti3C2 MXene fiber membrane prepared with different contents of Ti3C2 MXene in Example 2 of the present invention as a functional interlayer applied to a lithium-sulfur battery;

[0046] Fig.11 The Ti3C2 MXene fiber membranes with different Ti3C2 MXene contents in Example 2 of the present invention are used as functional interlayers in Cu / / Li batteries at 1 mA cm -2 Coulomb efficiency diagram below. DETAILED DESCRIPTION

[0047] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0048] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0049] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0050] The technical principle of the present invention is as follows:

[0051] The present invention provides a method for preparing a catalytic interlayer material for a lithium-sulfur battery, the method comprising:

[0052] S1. Multilayer Ti3C2T X After being dispersed in water, ultrasonic exfoliation was performed, followed by centrifugation, the upper suspension was collected and freeze-dried, and the dried product was ground to obtain a few-layer Ti3C2 MXene;

[0053] S2. dissolving polyacrylonitrile in N,N-dimethylformamide, and then adding the few-layer Ti3C2 MXene to obtain a mixed solution;

[0054] S3. Electrospinning is performed using the mixed solution as a raw material, and the obtained product is vacuum dried to obtain a Ti3C2MXene / PAN fiber membrane;

[0055] S4. The Ti3C2MXene / PAN fiber membrane is pre-oxidized by heating in an air atmosphere, and then carbonized at a high temperature in an argon atmosphere to obtain a porous Ti3C2MXene fiber membrane.

[0056] Step S1 specifically includes:

[0057] Multilayer Ti3C2T X Dispersed in water at a concentration of 2 mg / mL, placed in an ice bath at 350 W for ultrasonic exfoliation for 3 h, then centrifuged at 8000 r / min for 20 min, the upper suspension was collected and freeze-dried, the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene.

[0058] In the present invention, the purpose of passing the few-layer Ti3C2 MXene through a 400-mesh sieve is to remove large-sized MXene agglomerates that are difficult to grind after freeze-drying, and to obtain Ti3C2 MXene with uniform size dispersion.

[0059] Step S2 specifically includes:

[0060] Dissolving polyacrylonitrile in N,N-dimethylformamide, and then adding the few-layer Ti3C2 MXene to obtain a mixed solution;

[0061] Wherein, in the mixed solution, the concentration of polyacrylonitrile is 0.08±0.01 g / mL, and the content of the few-layer Ti3C2 MXene is 25-75wt%.

[0062] In the present invention, the content of the few-layer Ti3C2 MXene in the mixed solution is 25-75wt%. The purpose of regulating the structure and morphology of the interlayer material is achieved by regulating the content of the filler Ti3C2 MXene in the spinning solution and coordinating with the spinning processing conditions.

[0063] Step S3 specifically includes:

[0064] The mixed solution is used as a raw material for electrospinning, and the obtained product is vacuum dried at 60±5° C. for 12±2 h to obtain a Ti3C2 MXene / PAN fiber membrane;

[0065] Wherein, in the electrospinning process, the flow rate of the mixed solution is 0.4-1 mL / h, and the spinning voltage is set to 12-20 kV.

[0066] In the present invention, the flow rate of the mixed solution in the electrospinning process is 0.4-1 mL / h, and the spinning voltage is set to 12-20 kV. The advantage is that by regulating the spinning solution flow rate and the spinning voltage, fibers with uniform tube diameters can be obtained.

[0067] Step S4 specifically includes:

[0068] The Ti3C2 MXene / PAN fiber membrane was pre-oxidized by heating the Ti3C2 MXene / PAN fiber membrane to 250±10°C at 2°C / min in an air atmosphere for 1±0.5h, and then carbonized by heating the Ti3C2 MXene / PAN fiber membrane to 700±50°C at 5°C / min in an argon atmosphere for 1±0.2h to obtain a porous Ti3C2 MXene fiber membrane.

[0069] In the present invention, the purpose of pre-oxidation of the Ti3C2MXene / PAN fiber membrane is to enable PAN to maintain its structure after carbonization through the pre-oxidation step, thereby achieving the purpose of regulating the structural morphology of the sandwich material. The advantage of high-temperature carbonization at 700±50°C is that PAN can be further decomposed on the basis of maintaining the structural morphology of the sandwich material, thereby making the obtained sandwich material have higher conductivity.

[0070] The preparation method of a lithium-sulfur battery catalytic interlayer material and the catalytic interlayer material of the present application will be described in detail below in combination with examples and experimental data.

[0071] Example 1

[0072] This embodiment provides a method for preparing a catalytic interlayer material for a lithium-sulfur battery. Figure 1 As shown, specifically including:

[0073] Step S1: Figure 1 As shown in a, the multilayer Ti3C2T X Disperse in ultrapure water at a concentration of 2 mg / mL, place in an ice bath at 350 W power for ultrasonic stripping for 3 h, centrifuge the suspension at 8000 r / min for 20 min, collect the upper suspension and freeze-dry, grind the freeze-dried few-layer Ti3C2MXene and sieve through 400 mesh to obtain the few-layer Ti3C2MXene for use;

[0074] Step S2: 0.666 g of PAN (polyacrylonitrile) was placed in a reagent bottle, and then 8 mL of N,N-dimethylformamide was added, and stirred at 60° C. until it was completely dissolved;

[0075] Step S3: adding different contents of few-layer Ti3C2MXene to the above-mentioned N,N-dimethylformamide solution containing PAN, stirring at 60°C for 2h to obtain mixed solutions with Ti3C2MXene contents of 0wt%, 25wt%, 50wt% and 75wt%, respectively. Figure 1 As shown in b;

[0076] Step S4: Figure 1c, the above mixed solution was added to the injection pump, and the spinning was performed by adjusting the flow rate of the mixed solution (0.4, 0.6, 0.8, 1 mL / h) and the spinning voltage (12, 16, 20 kV). Then the sample was placed in a vacuum drying oven at 60 °C and dried for 12 h to obtain Ti3C2 MXene / PAN fiber membranes with different fiber sizes. The structural morphology of the membranes is shown in Figure 2 As shown ( Figure 2 ac, Ti3C2 MXene / PAN presents a good three-dimensional network structure, and the fiber size increases significantly with the Ti3C2 MXene content from 0 to 50wt%, but when the Ti3C2MXene content reaches 75wt%, a large number of blocky Ti3C2MXene appear, indicating that the three-dimensional network structure cannot be maintained at this content. Therefore, from the morphological point of view, the Ti3C2 MXene content of 50wt% is closer to the critical value of morphology control);

[0077] Step S5: The Ti3C2 MXene / PAN fiber membrane is placed in a tube furnace, heated to 250°C at 2°C / min in air atmosphere for pre-oxidation for 1 h, and then heated to 700°C at 5°C / min in argon atmosphere for carbonization for 1 h (see Figure 1 d), and obtained porous Ti3C2 MXene fiber membranes of different sizes, the SEM images of which are shown in Figure 3 As shown;

[0078] Step S6: Cut the porous Ti3C2 MXene fiber membrane into discs with a diameter of 19 mm, as shown in the figure Figure 4 As shown, it is used as a functional interlayer and assembled with the positive electrode shell, positive electrode, separator, lithium sheet, gasket, spring and negative electrode shell to form a lithium-sulfur battery system. The assembly diagram and the mechanism of action of the functional interlayer are shown in Figure 1 As shown in e.

[0079] Example 2

[0080] In this example, the interlayer material prepared in Example 1 is characterized and its performance is tested.

[0081] 1. Structural morphology characterization of Ti3C2 MXene before and after exfoliation. Figure 5 SEM images of Ti3C2 MXene before and after exfoliation. Figure 5 a It can be seen that the Ti3C2 MXene before exfoliation is a typical multilayer structure, in the shape of an "accordion", and the Ti3C2 MXene after exfoliation presents a few-layer structure, confirming the successful exfoliation of Ti3C2 MXene.

[0082] 2. XRD patterns of Ti3C2 MXene before and after peeling, see Figure 6As shown in the figure, after exfoliation, the peak position of the 002 crystal plane representing MXene shifts to the left. According to the Bragg equation 2ds inθ=nλ, the interlayer spacing of MXene increases after exfoliation, which confirms the successful exfoliation of MXene.

[0083] 3. Figure 7 The cycling performance spectrum of lithium-sulfur battery with Ti3C2 MXene fiber membrane with 50wt% Ti3C2 MXene content as functional interlayer under 0.2C high load. It can be seen from the figure that when the sulfur loading is 9.47mg cm -2 and 5.40 mg cm -2 When the functional interlayer of this embodiment is added, the initial surface capacity of the battery after 100 cycles at 0.2C is 7.17 and 5.09 mA h cm -2, , the retention rates reached 90.3% and 80.7% respectively, and they still had good performance even in the case of low electrolyte and high sulfur loading, proving that the Ti3C2 MXene fiber membrane functional interlayer can not only effectively inhibit the shuttle of polysulfides but also accelerate the redox kinetics of sulfur. Therefore, the battery introducing the functional interlayer can present a higher surface capacity and stable cycle performance.

[0084] 4. Figure 8 The graph shows the cycling stability performance test of Ti3C2 MXene fiber membranes with different Ti3C2 MXene contents as functional interlayers in lithium-sulfur batteries at 0.5C. As can be seen from the figure, with the change of Ti3C2 MXene content (0, 25, 50 and 75wt%), the corresponding initial specific capacities are 917.9, 1053.8, 1140.8 and 1084.3 mA h g -1 After 100 cycles, there are still 86.3%, 84.3%, 87.7% and 85.2% capacity retention rates, indicating that the Ti3C2MXene fiber membrane functional interlayer material has a significant catalytic effect, and the functional interlayer with a Ti3C2MXene content of 50wt% has the best catalytic effect, and the corresponding lithium-sulfur battery has good cycle performance.

[0085] 5. Fig. 9 The 2C cycle stability spectrum of Ti3C2 MXene fiber membrane functional interlayer with Ti3C2 MXene content of 0wt.% and 50wt.% applied to lithium-sulfur batteries. As can be seen from the figure, the capacity retention rate of the functional interlayer with Ti3C2MXene content of 50wt% after 200, 400, and 600 cycles is 76.2%, 65.5%, and 58.0%, respectively, proving that the strong anchoring effect and efficient catalytic ability of Ti3C2 MXene fiber membrane on lithium polysulfide can effectively improve the cycle stability of the battery.

[0086] 6. Fig.10 The figure shows the rate performance spectrum of Ti3C2 MXene fiber membranes with different Ti3C2 MXene contents as functional interlayers in lithium-sulfur batteries. As can be seen from the figure, at 0.2, 0.5, 1, 2, and 3C, the reversible discharge specific capacity of the fiber membrane with a Ti3C2 MXene content of 50wt% as a functional interlayer is 1292.010, 1165.411, 1067.398, 944.465 and 867.286mA h g -1 When the discharge current returns to 0.2C, its reversible discharge capacity returns to 1217.021mA hg -1 , indicating that Ti3C2MXene fiber membrane has good capacity and stability at different rates.

[0087] 7. Fig.11 Ti3C2 MXene fiber membranes with different Ti3C2 MXene contents were used as functional interlayers in Cu / / Li batteries at 1 mA cm -2 The coulombic efficiency diagram below. As can be seen from the figure, the coulombic efficiency (CE) of the battery with a functional interlayer of 0 and 50wt% Ti3C2MXene added remained basically unchanged after 100 cycles, indicating that the MXene fiber membrane can effectively promote the reversible lithium removal and lithium insertion process.

[0088] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0089] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0090] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a catalytic interlayer material for a lithium-sulfur battery, characterized in that: The preparation method comprises: Multilayer Ti3C2T X After being dispersed in water, ultrasonic exfoliation was performed, followed by centrifugation, the upper suspension was collected and freeze-dried, and the dried product was ground to obtain a few-layer Ti3C2 MXene; Dissolving polyacrylonitrile in N,N-dimethylformamide, and then adding the few-layer Ti3C2 MXene to obtain a mixed solution; The mixed solution is used as a raw material for electrospinning, and the obtained product is vacuum dried to obtain a Ti3C2 MXene / PAN fiber membrane; The Ti3C2 MXene / PAN fiber membrane is pre-oxidized by heating in an air atmosphere, and then carbonized at a high temperature in an argon atmosphere to obtain a porous Ti3C2 MXene fiber membrane.

2. The method for preparing a lithium-sulfur battery catalytic interlayer material according to claim 1, characterized in that: The multilayer Ti3C2T X After being dispersed in water, ultrasonic peeling is performed, followed by centrifugation, the upper suspension is collected and freeze-dried, and the dried product is ground to obtain a few-layer Ti3C2 MXene, which specifically includes: Multilayer Ti3C2T X Dispersed in water at a concentration of 2 mg / mL, subjected to ultrasonic exfoliation and centrifugation, the upper suspension was collected and freeze-dried, and the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene.

3. The method for preparing a lithium-sulfur battery catalytic interlayer material according to claim 2, characterized in that: The multilayer Ti3C2T X Dispersed in water at a concentration of 2 mg / mL, subjected to ultrasonic exfoliation and centrifugation, the upper suspension was collected and freeze-dried, the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene, specifically comprising: Multilayer Ti3C2T X Dispersed in water at a concentration of 2 mg / mL, placed in an ice bath at 350 W for ultrasonic exfoliation for 3 h, then centrifuged at 8000 r / min for 20 min, the upper suspension was collected and freeze-dried, the dried product was ground and passed through a 400-mesh sieve to obtain a few-layer Ti3C2 MXene.

4. The method for preparing a lithium-sulfur battery catalytic interlayer material according to claim 1, characterized in that: The method of dissolving polyacrylonitrile in N,N-dimethylformamide and then adding the few-layer Ti3C2 MXene to obtain a mixed solution specifically comprises: Dissolving polyacrylonitrile in N,N-dimethylformamide, and then adding the few-layer Ti3C2 MXene to obtain a mixed solution; Wherein, in the mixed solution, the concentration of polyacrylonitrile is 0.08±0.01 g / mL, and the content of the few-layer Ti3C2 MXene is 25-75wt%.

5. The method for preparing a lithium-sulfur battery catalytic interlayer material according to claim 1, characterized in that: The electrospinning is performed using the mixed solution as a raw material, and the obtained product is vacuum dried to obtain a Ti3C2MXene / PAN fiber membrane, which specifically includes: The mixed solution is used as a raw material for electrospinning, and the obtained product is vacuum dried at 60±5° C. for 12±2 h to obtain a Ti3C2 MXene / PAN fiber membrane; Wherein, in the electrospinning process, the flow rate of the mixed solution is 0.4-1 mL / h, and the electrospinning voltage is 12-20 kV.

6. The method for preparing a lithium-sulfur battery catalytic interlayer material according to claim 1, characterized in that: The Ti3C2 MXene / PAN fiber membrane is pre-oxidized by heating in an air atmosphere, and then carbonized at a high temperature in an argon atmosphere to obtain a porous Ti3C2 MXene fiber membrane, which specifically includes: The Ti3C2 MXene / PAN fiber membrane was pre-oxidized by heating the Ti3C2 MXene / PAN fiber membrane to 250±10°C at 2°C / min in an air atmosphere for 1±0.5h, and then carbonized by heating the Ti3C2 MXene / PAN fiber membrane to 700±50°C at 5°C / min in an argon atmosphere for 1±0.2h to obtain a porous Ti3C2 MXene fiber membrane.

7. A lithium-sulfur battery catalytic interlayer material, characterized in that: The catalytic interlayer material is prepared by the preparation method of a catalytic interlayer material for a lithium-sulfur battery according to any one of claims 1-6.

8. A lithium-sulfur battery, characterized in that: The lithium-sulfur battery comprises a lithium-sulfur battery catalytic interlayer material as described in claim 7.

9. A method for preparing a lithium-sulfur battery as claimed in claim 8, characterized in that: The preparation method comprises: Cutting the lithium-sulfur battery catalytic interlayer material according to claim 7 into discs with a diameter of 19 mm to obtain a lithium-sulfur battery interlayer; The lithium-sulfur battery interlayer is assembled with the positive electrode shell, the positive electrode, the separator, the lithium sheet, the gasket, the shrapnel and the negative electrode shell to form a lithium-sulfur battery.

Citation Information

Patent Citations

  • Preparation method of cathode functional interlayer applied to lithium-sulfur battery

    CN107732104A

  • Preparation and application of anode carbon-based membrane material for lithium-sulfur battery

    CN113555547A