Perovskite thin film and preparation method thereof, perovskite cell and preparation method thereof

By introducing volatile ammonium salt additives in the preparation process of perovskite films, pores are formed to promote the reaction between organic salts and inorganic salts, the problem of incomplete lead iodide reaction in perovskite films is solved, and the film and Battery performance.

CN118984638APending Publication Date: 2024-11-19TRINA SOLAR CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411078143.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the preparation process of the existing perovskite film, the lead iodide in the inorganic salt skeleton layer reacts thoroughly with the organic salt, which affects product performance.

Method used

In the process of evaporating the preparation of the inorganic salt skeleton layer, volatile ammonium salt additives are introduced to evaporate and leave during the first annealing treatment, forming pores, promoting subsequent penetration and reaction of organic salts, and ensuring the complete reaction of lead iodide. And promote the growth of perovskite crystal nuclei.

Benefits of technology

Effectively adjust the film formation quality of perovskite films and improve the performance of perovskite films and batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984638A_ABST
    Figure CN118984638A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of perovskite batteries, and particularly provides a perovskite thin film and a preparation method thereof, and a perovskite battery and a preparation method thereof. The objective of the invention is to solve the problem that lead iodide in an inorganic salt skeleton layer does not react thoroughly with organic salt in the preparation process of an existing perovskite thin film, so that the product performance is affected. Therefore, the preparation method comprises the following steps that an inorganic salt framework layer containing an additive is prepared on the surface of a base material through first evaporation operation, then first annealing treatment is conducted, and the inorganic salt framework layer internally provided with a plurality of pores is obtained on the surface of the base material; preparing an organic layer on the surface of the inorganic salt skeleton layer with a plurality of pores inside through second evaporation operation, and then carrying out second annealing treatment to obtain a perovskite thin film on the surface of the substrate; wherein the additive comprises an ammonium salt additive capable of volatilizing in the first annealing treatment. According to the preparation method of the perovskite thin film, lead iodide can react completely, and the performance of a perovskite battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of perovskite cells, and specifically provides a perovskite film and a preparation method thereof, a perovskite cell and a preparation method thereof. Background Art

[0002] As an important preparation technology for perovskite solar cells (PSCs), the evaporation method for preparing perovskite thin films has made significant progress in recent years. Researchers have continuously optimized the evaporation process parameters, such as deposition rate, substrate temperature, atmosphere control, etc., and have successfully achieved the preparation of high-efficiency perovskite films and constructed high-efficiency perovskite solar cells based on this.

[0003] Vacuum evaporation is promising for the fabrication of scalable perovskite solar cells. However, the poor thermal conductivity of metal halide powders leads to unfavorable temperature non-uniformity, which destroys the stability of the evaporation rate and poses a major challenge to the repeatable deposition of perovskite films. Chenyi Yi from Tsinghua University reported a molten salt sequential evaporation strategy that can be used to reproducibly fabricate efficient FA-based perovskite solar cells with good stability. This method can form molten salts at temperatures far below the melting points of metal halides by mixing metal halides in a certain proportion. Compared with traditional multi-source co-evaporation methods, the molten salt strategy can greatly simplify the evaporation process. Compared with solid lead halide powders, liquid molten salts can greatly uniform the temperature, and their evaporation rate can remain stable throughout the evaporation cycle, greatly improving the batch-to-batch stability of evaporation.

[0004] Although the above method of regulating the inorganic salt skeleton layer by evaporating the molten metal salt can simplify the evaporation step, the material composition is difficult to accurately control and cannot have a favorable effect on the subsequent deposition of the organic salt. In the process of reacting with the organic salt, there is a problem of incomplete reaction between the lead iodide in the inorganic salt skeleton layer and the organic salt, which affects the product performance.

[0005] Accordingly, this field requires a new technical solution to solve the above technical problems. Summary of the invention

[0006] The present application aims to solve the above technical problem, that is, to solve the problem that in the preparation process of the existing perovskite film, the lead iodide in the inorganic salt skeleton layer does not react completely with the organic salt, thereby affecting the product performance.

[0007] In a first aspect, the present application provides a method for preparing a perovskite film, which comprises the following steps: preparing an inorganic salt skeleton layer containing an additive on the surface of a substrate by a first evaporation operation, and then performing a first annealing treatment to obtain an inorganic salt skeleton layer having a plurality of pores inside on the surface of the substrate; preparing an organic layer on the surface of the inorganic salt skeleton layer having a plurality of pores inside by a second evaporation operation, and then performing a second annealing treatment to obtain a perovskite film on the surface of the substrate; wherein the additive comprises at least an ammonium salt additive that can volatilize during the first annealing treatment.

[0008] In the preferred technical solution of the above-mentioned method for preparing the perovskite film, the ammonium salt additive includes at least one of ammonium formate, ammonium acetate, ammonium chloride and ammonium trifluoroacetate.

[0009] In the preferred technical solution of the above-mentioned method for preparing the perovskite thin film, the evaporation source in the first evaporation operation includes a first evaporation source, a second evaporation source and a third evaporation source, the first evaporation source includes at least lead iodide, the second evaporation source includes at least at least one of cesium bromide and cesium iodide, and the third evaporation source includes at least the ammonium salt additive.

[0010] In the preferred technical solution of the above-mentioned method for preparing the perovskite thin film, in the first evaporation operation, the evaporation rate of the first evaporation source is The evaporation rate of the second evaporation source is (0.3-0.5) : 1; and / or, in the first evaporation operation, the evaporation rate of the first evaporation source is The evaporation rate of the third evaporation source: the evaporation rate of the first evaporation source is (0.001-0.05):1.

[0011] In the preferred technical scheme of the above-mentioned method for preparing the perovskite film, in the first evaporation operation, the evaporation thickness of the inorganic salt skeleton layer is 200 to 310 nm; and / or, in the process of the first annealing treatment, the annealing temperature is 150 to 250° C., and the annealing time is 5 to 30 min.

[0012] In the preferred technical solution of the above-mentioned method for preparing the perovskite thin film, the evaporation source in the second evaporation operation includes at least one of formamidine iodide, formamidine bromide, formamidine chloride, methylamine iodide, methylamine bromide, and methylamine chloride; and / or, in the second evaporation operation, the evaporation rate of the evaporation source is And / or, in the second evaporation operation, the evaporation thickness of the organic layer is 250-350 nm.

[0013] In the preferred technical scheme of the above-mentioned method for preparing the perovskite film, the second annealing treatment includes a first annealing stage and a second annealing stage performed sequentially, the first annealing stage is specifically annealing in an inert gas atmosphere in a glove box, the annealing temperature is 130-160°C, and the annealing time is 3-20min; the second annealing stage is annealing in air with a humidity RH of 30%-40%, the annealing temperature is 130-150°C, and the annealing time is 10-60min.

[0014] In a second aspect, the present application provides a perovskite film, which is prepared by the above-mentioned perovskite film preparation method.

[0015] In a third aspect, the present application provides a perovskite cell, wherein the perovskite cell comprises the above-mentioned perovskite film.

[0016] In a fourth aspect, the present application provides a method for preparing a perovskite battery, which comprises the following steps: preparing a hole transport layer on the conductive side surface of a transparent conductive substrate to obtain a substrate; preparing a perovskite film on the surface of the hole transport layer of the substrate using the above-mentioned perovskite film preparation method; preparing a passivation material layer on the surface of the perovskite film by a third evaporation operation, and then performing a third annealing treatment to obtain a passivation layer; preparing an electron transport layer on the surface of the passivation layer; preparing a buffer layer on the surface of the electron transport layer; and preparing an electrode layer on the surface of the buffer layer.

[0017] In the preferred technical scheme of the preparation method of the above-mentioned perovskite battery, the hole transport layer includes a first material layer and a second material layer sequentially superimposed on the transparent conductive substrate, the material of the first material layer is nickel oxide, and the material of the second material layer includes at least one of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid, [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], and 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline.

[0018] In the preferred technical solution of the above-mentioned perovskite battery preparation method, the hole transport layer is prepared by any one of spin coating, slit coating, magnetron sputtering or evaporation; and / or the thickness of the hole transport layer is 1 to 50 nm.

[0019] In the preferred technical solution of the above-mentioned method for preparing a perovskite cell, the first material layer is prepared by magnetron sputtering, and the second material layer is prepared by spin coating.

[0020] In the preferred technical scheme of the above-mentioned method for preparing the perovskite battery, the evaporation source of the third evaporation operation is at least one of iodinated phenylethylamine, 4-trifluoromethyl-aniline iodide, 2-thiopheneethylamine iodide, ethylamine salt iodide, and guanidine iodide; and / or, in the third evaporation operation, the evaporation rate of the evaporation source is And / or, in the third evaporation operation, the evaporation thickness of the passivation material layer is 1 to 10 nm; and / or, the third annealing treatment is specifically annealing in an inert gas atmosphere in a glove box, with an annealing temperature of 60 to 120° C. and an annealing time of 1 to 5 min.

[0021] In the preferred technical scheme of the preparation method of the above-mentioned perovskite battery, the material of the electron transport layer is any one of fullerene and its derivatives; and / or, the material of the buffer layer is one of bathocuproin or atomic layer deposited tin dioxide; and / or, the material of the electrode layer is any one of metal electrode silver, metal electrode copper, transparent conductive oxide ITO, indium zinc oxide, tungsten-doped indium oxide and aluminum-doped zinc oxide.

[0022] Compared with the prior art, the beneficial effects of this application are:

[0023] The preparation method of the perovskite film of the present application introduces a volatile ammonium salt additive during the process of preparing the inorganic salt skeleton layer by evaporation, so that the inorganic salt skeleton layer obtained by evaporation contains the ammonium salt additive. During the first annealing treatment, the ammonium salt additive evaporates and leaves, and forms a number of pores in the inorganic salt skeleton layer during the outward volatilization process, which is beneficial to the subsequent penetration and reaction of the organic salt, so that the lead iodide in the inorganic salt skeleton layer reacts thoroughly, and the perovskite crystal nucleus can grow smoothly, which can effectively adjust the film formation quality of the perovskite film and improve the performance of the perovskite film and the performance of the perovskite battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The preferred embodiments of the present application are described below in conjunction with the accompanying drawings, in which:

[0025] Figure 1 is a flow chart of a method for preparing a perovskite film according to an embodiment of the present application;

[0026] Figure 2 is a schematic structural diagram of a perovskite battery in an embodiment of the present application;

[0027] Figure 3 It is a flow chart of a method for preparing a perovskite battery according to an embodiment of the present application.

[0028] List of reference numerals:

[0029] 1. Transparent conductive substrate; 2. Hole transport layer; 3. Perovskite film; 4. Passivation layer; 5. Electron transport layer; 6. Buffer layer; 7. Electrode layer. DETAILED DESCRIPTION

[0030] The preferred embodiments of the present application are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present application and are not intended to limit the protection scope of the present application.

[0031] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0032] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0033] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0034] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0035] The experimental methods in the following examples are conventional methods unless otherwise specified, and the materials, reagents, etc. used in the following examples are commercially available unless otherwise specified.

[0036] As pointed out in the background art, in the preparation process of the existing perovskite thin film, the lead iodide in the inorganic salt skeleton layer does not react completely with the organic salt, which affects the product performance.

[0037] The preparation method of the perovskite film of the present application introduces a volatile ammonium salt additive during the process of preparing the inorganic salt skeleton layer by evaporation, so that the inorganic salt skeleton layer obtained by evaporation contains the ammonium salt additive. During the first annealing treatment, the ammonium salt additive evaporates and leaves, thereby leaving a number of pores in the inorganic salt skeleton layer, which is beneficial to the subsequent penetration and reaction of the organic salt, so that the lead iodide in the inorganic salt skeleton layer reacts thoroughly, and the perovskite crystal nucleus can grow smoothly, which can effectively adjust the film quality of the perovskite film and improve the performance of the perovskite film and the performance of the perovskite battery.

[0038] In a first aspect, the present application provides a method for preparing a perovskite film, see Figure 1 The method for preparing the perovskite film comprises the following steps:

[0039] S1: preparing an inorganic salt skeleton layer containing additives on the surface of the substrate by a first evaporation operation, and then performing a first annealing treatment to obtain an inorganic salt skeleton layer having a plurality of pores inside on the surface of the substrate, wherein the additives at least include an ammonium salt additive that can volatilize during the first annealing treatment.

[0040] By introducing a volatile ammonium salt additive during the process of preparing an inorganic salt skeleton layer by evaporation, the inorganic salt skeleton layer obtained by evaporation contains the ammonium salt additive. During the first annealing treatment, the ammonium salt additive evaporates and leaves after being heated. In the process of volatilization, a number of pores are formed in the inorganic salt skeleton layer, which is conducive to the subsequent penetration and reaction of organic salts, thereby allowing the lead iodide in the inorganic salt skeleton layer to react completely, and at the same time helping the perovskite crystal nucleus to grow smoothly, and can effectively adjust the film formation quality of the perovskite film.

[0041] S2: preparing an organic layer on the surface of the inorganic salt skeleton layer having a plurality of pores inside by a second evaporation operation, and then performing a second annealing treatment to obtain a perovskite film on the surface of the substrate. The perovskite film is a perovskite absorption layer formed by the organic salt of the organic layer penetrating into the inorganic salt skeleton layer and the organic salt reacting with the inorganic salt so that the organic layer and the inorganic salt skeleton layer are combined.

[0042] The organic salt in the organic layer can penetrate into the inorganic salt skeleton layer through several pores, so that the organic salt fully reacts with lead iodide during the second annealing process, causing the lead iodide in the inorganic salt skeleton layer to react completely, effectively avoiding residual lead iodide in the inorganic salt skeleton layer, thereby improving the performance of the perovskite film and the performance of the perovskite battery.

[0043] The preparation method of the perovskite film of the present application introduces a volatile ammonium salt additive into the inorganic salt skeleton layer during the preparation of the inorganic salt skeleton layer, so that the ammonium salt additive can leave pores in the inorganic salt skeleton layer after volatilization in the first annealing treatment stage, which is beneficial for the subsequent penetration of organic salts and reaction with inorganic salts, thereby effectively regulating the deposition process of the film and improving the repeatability between batches.

[0044] It should be noted that the present application does not impose any restrictions on the specific composition of the ammonium salt additive, as long as the ammonium salt additive can volatilize during the first annealing treatment, thereby forming a number of pores in the inorganic salt skeleton layer. In practical applications, technicians in this field can set the specific composition of the ammonium salt additive according to actual needs.

[0045] Optionally, the ammonium salt additive includes at least one of ammonium formate, ammonium acetate, ammonium chloride, and ammonium trifluoroacetate.

[0046] In some embodiments, in step S1, the evaporation source in the first evaporation operation includes a first evaporation source, a second evaporation source and a third evaporation source, wherein the first evaporation source includes at least lead iodide, the second evaporation source includes at least one of cesium bromide and cesium iodide, and the third evaporation source includes at least an ammonium salt additive.

[0047] Co-evaporation is performed through a first evaporation source, a second evaporation source and a third evaporation source to prepare an inorganic salt skeleton layer containing additives on the surface of the substrate, which is convenient to operate and easy to control.

[0048] In some embodiments, the evaporation rate of the first evaporation source is The evaporation rate of the second evaporation source: the evaporation rate of the first evaporation source is (0.3~0.5):1.

[0049] By setting it in this way, the evaporation rate of the second evaporation source is controlled within a certain proportional range relative to the evaporation rate of lead iodide, which can better control the component content of the inorganic salt skeleton layer obtained by evaporation, and help improve the performance of the perovskite film.

[0050] In some embodiments, the evaporation rate of the first evaporation source is The evaporation rate of the third evaporation source: the evaporation rate of the first evaporation source is (0.001~0.05):1.

[0051] By such a setting, the evaporation rate of the ammonium salt additive is controlled within a certain proportional range relative to the evaporation rate of lead iodide, so that the ammonium salt additive can be evenly distributed in the inorganic salt skeleton layer, and the amount of the introduced ammonium salt additive can be effectively controlled, thereby controlling the number and size of pores in the final organic salt skeleton layer and making a number of pores evenly distributed in the inorganic salt skeleton layer, so that the subsequent organic salt can evenly penetrate into various regions for reaction.

[0052] In some embodiments, in step S1, in the first evaporation operation, the evaporation thickness of the inorganic salt skeleton layer is 200-310 nm.

[0053] Controlling the evaporation thickness of the inorganic salt skeleton layer to 200-310 nm can effectively control the content of the inorganic salt, thereby improving the performance of the perovskite film.

[0054] In some embodiments, in step S1, during the first annealing treatment, the annealing temperature is 150-250° C., and the annealing time of the first annealing treatment is 5-30 min.

[0055] The annealing temperature of the first annealing treatment is set at 150-250° C. and the annealing time of the first annealing treatment is set at 5-30 min, so that the ammonium salt additive can be stably volatilized and the inorganic salt skeleton layer can be stably formed.

[0056] Optionally, the evaporation source in the second evaporation operation includes at least one of formamidine iodide, formamidine bromide, formamidine chloride, methylamine iodide, methylamine bromide, and methylamine chloride.

[0057] In some embodiments, the evaporation rate of the evaporation source in the second evaporation operation is

[0058] In some preferred embodiments, the evaporation rate of the evaporation source in the second evaporation operation is

[0059] By controlling the evaporation rate of the evaporation source in the second evaporation operation, the deposition process of the organic salt can be controlled, so that the organic salt is uniformly deposited to obtain a uniform organic layer.

[0060] In some embodiments, in step S2, in the second evaporation operation, the evaporation thickness of the organic layer is 250-350 nm.

[0061] Controlling the evaporation thickness of the organic layer to 250-350 nm can effectively control the content of organic salts and help improve the performance of the perovskite film.

[0062] In some embodiments, in step S2, the second annealing treatment includes a first annealing stage and a second annealing stage performed sequentially. The first annealing stage is specifically annealing in an inert gas atmosphere in a glove box, the annealing temperature is 130-160°C, and the annealing time is 3-20 minutes; the second annealing stage is annealing in air with a humidity RH of 30%-40%, the annealing temperature is 130-150°C, and the annealing time is 10-60 minutes.

[0063] The second annealing treatment is divided into two steps. The first step is annealing in a glove box to preliminarily solidify the organic layer. Then, the second step is annealing in air with a certain humidity to allow the organic salt to penetrate smoothly and react with the inorganic salt, so as to obtain a perovskite film with a smooth interface and uniform perovskite crystal nuclei.

[0064] In a second aspect, the present application provides a perovskite film, which is prepared by the method for preparing a perovskite film provided in the first aspect.

[0065] In a third aspect, the present application provides a perovskite cell, wherein the perovskite cell comprises the perovskite film provided in the second aspect.

[0066] In a fourth aspect, the present application provides a method for preparing a perovskite battery, see Figure 3 , the preparation method of the perovskite battery comprises the following steps:

[0067] S100: preparing a hole transport layer on the conductive side surface of a transparent conductive substrate to obtain a substrate.

[0068] S210: preparing an inorganic salt skeleton layer containing additives on the surface of the substrate through a first evaporation operation; then performing a first annealing treatment to obtain an inorganic salt skeleton layer having a plurality of pores inside on the surface of the substrate.

[0069] S220: preparing an organic layer on the surface of the inorganic salt skeleton layer having a plurality of pores inside by a second evaporation operation, and then performing a second annealing treatment to obtain a perovskite film on the surface of the substrate.

[0070] S300: preparing a passivation material layer on the surface of the perovskite film through a third evaporation operation, and then performing a third annealing treatment to obtain a passivation layer.

[0071] S400: preparing an electron transport layer on the surface of the passivation layer.

[0072] S500: preparing a buffer layer on the surface of the electron transport layer.

[0073] S600: preparing an electrode layer on the surface of the buffer layer.

[0074] In some embodiments, the hole transport layer includes a first material layer and a second material layer sequentially stacked on a transparent conductive substrate. Optionally, the material of the first material layer is nickel oxide, and the material of the second material layer includes at least one of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid (4PADCB), poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), and 4,4'-cyclohexylbis[N,N-bis(4-methylphenyl)aniline (TAPC).

[0075] Optionally, the hole transport layer is prepared by any one of spin coating, slit coating, magnetron sputtering or evaporation.

[0076] In some embodiments, the thickness of the hole transport layer is 1-50 nm. The thickness of the hole transport layer is controlled to be 1-50 nm to ensure the performance of the perovskite cell.

[0077] In one embodiment, the first material layer is made by magnetron sputtering, and the second material layer is made by spin coating. The first material layer is made by magnetron sputtering, and the second material layer is made by spin coating, so that the performance of the prepared hole transport layer is better.

[0078] In some embodiments, in step S300, the evaporation source of the third evaporation operation is at least one of phenylethylamine iodide (PEAI), 4-trifluoromethyl-phenylamine iodate (CF3-PAI), 2-thiopheneethylamine iodate (TEAI), ethylamine salt iodate (EAI), and guanidine iodide (GUAl).

[0079] In some embodiments, in step S300, in the third evaporation operation, the evaporation rate of the evaporation source is

[0080] In some embodiments, in step S300, in the third evaporation operation, the evaporation thickness of the passivation material layer is 1-10 nm.

[0081] In some embodiments, in step S300, the third annealing treatment is specifically performed in an inert gas atmosphere in a glove box, with an annealing temperature of 60 to 120°C and an annealing time of 1 to 5 minutes.

[0082] Optionally, the material of the electron transport layer is fullerene and its derivatives (C 60 , C 70 , PCBM) any one.

[0083] Optionally, the material of the buffer layer is one of bathocuproine (BCP) or atomic layer deposited tin dioxide (SnO2).

[0084] Optionally, the material of the electrode layer is any one of metal electrode silver (Ag), metal electrode copper (Cu), transparent conductive oxide ITO, indium zinc oxide (IZO), tungsten-doped indium oxide (IWO) and aluminum-doped zinc oxide (AZO).

[0085] The following is a detailed description of the perovskite film and perovskite battery of the present application through several specific embodiments. Figure 2 The perovskite battery in the embodiment includes, from bottom to top, a transparent conductive substrate 1, a hole transport layer 2, a perovskite film 3, a passivation layer 4, an electron transport layer 5, a buffer layer 6 and an electrode layer 7.

[0086] Example 1

[0087] The perovskite battery of this embodiment is prepared by the following steps:

[0088] S100: NiOx was deposited on a transparent conductive substrate by magnetron sputtering with a thickness of 30 nm. Self-assembled material 2PACz was deposited on the surface of NiOx by spin coating. 2PACz was dissolved in ethanol with a concentration of 0.05 mg / mL. The spin coating speed was 4000 rpm / s, the spin coating thickness was 5 nm, and annealing was performed at 100°C for 10 min. A substrate with a hole transport layer was obtained.

[0089] S210: ammonium formate (NH4fa), lead iodide (PbI2) and cesium bromide (CsBr) are co-evaporated on the surface of the hole transport layer of the substrate by evaporation to obtain an inorganic salt skeleton layer containing the additive NH4fa (PbI2 and CsBr skeleton layer containing NH4fa), wherein the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is The total evaporated thickness of the inorganic salt skeleton layer is 255 nm. Then, it is annealed in a N2 atmosphere at a temperature of 175° C. for 30 min to obtain an inorganic salt skeleton layer with several pores.

[0090] S220: Depositing an organic layer on the surface of an inorganic salt skeleton layer having a plurality of pores by evaporation, wherein the evaporation source is potassium amidine iodide (FAI), and the evaporation rate of FAI is The evaporation thickness of the organic layer is 280nm; then, annealing is carried out in a N2 atmosphere in a glove box at a temperature of 130°C for 5 minutes to obtain a prefabricated perovskite layer; the prefabricated perovskite layer is annealed again in air with a humidity RH of 30%-40% at a temperature of 150°C for 20 minutes to obtain a perovskite film (i.e., a perovskite absorption layer).

[0091] S300: 2-thiopheneethylamine iodate (TEAI) is evaporated on the surface of the perovskite absorption layer by evaporation to obtain a passivation material layer, wherein TEAI powder is placed in a linear evaporation source and the temperature is slowly increased until the rate reaches The baffle was turned on for evaporation, and the evaporation thickness of the passivation material layer was 2 nm. Then, annealing was performed in a N2 atmosphere in a glove box at a temperature of 80° C. for 5 min to obtain a passivation layer.

[0092] S400: 20nm electron transport layer C is deposited on the surface of the passivation layer by evaporation method 60 .

[0093] S500: Using evaporation method on the electron transport layer C 60 A 5nm buffer layer BCP is evaporated on the surface.

[0094] S600: A Ag metal electrode layer with a thickness of 100 nm is prepared on the surface of the buffer layer by a thermal evaporation method to obtain a perovskite cell.

[0095] Example 2

[0096] The preparation method of the perovskite battery in this embodiment is the same as that in Embodiment 1, and the only difference from Embodiment 1 is that in step S200, the ammonium salt additive is ammonium chloride.

[0097] Example 3

[0098] The preparation method of the perovskite battery in this embodiment is the same as that in Embodiment 1, and the only difference from Embodiment 1 is that in step S200, the ammonium salt additive is ammonium trifluoroacetate, and cesium bromide is replaced by cesium iodide.

[0099] Example 4

[0100] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 1, and the only difference from embodiment 1 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0101] Example 5

[0102] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 1, and the only difference from embodiment 1 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0103] Example 6

[0104] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0105] Example 7

[0106] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0107] Example 8

[0108] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0109] Example 9

[0110] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0111] Example 10

[0112] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0113] Embodiment 11

[0114] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0115] Example 12

[0116] The preparation method of the perovskite battery in this embodiment is the same as that in embodiment 4, and the only difference from embodiment 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0117] Comparative Example 1

[0118] The preparation method of the perovskite battery in this comparative example is the same as that in Example 1, the only difference from Example 1 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0119] Comparative Example 2

[0120] The preparation method of the perovskite battery in this comparative example is the same as that in Example 1, the only difference from Example 1 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0121] Comparative Example 3

[0122] The preparation method of the perovskite battery in this comparative example is the same as that in Example 4, and the only difference from Example 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0123] Comparative Example 4

[0124] The preparation method of the perovskite battery in this comparative example is the same as that in Example 4, and the only difference from Example 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0125] Comparative Example 5

[0126] The preparation method of the perovskite battery in this comparative example is the same as that in Example 4, and the only difference from Example 4 is that in step S200, the evaporation source does not include an ammonium salt additive.

[0127] Comparative Example 6

[0128] The preparation method of the perovskite battery in this comparative example is the same as that in Example 4, and the only difference from Example 4 is that in step S200, the evaporation rate of PbI2 is The evaporation rate of CsBr is The evaporation rate of NH4fa is

[0129] The perovskite cells prepared in Examples 1 to 12 and Comparative Examples 1 to 6 were respectively subjected to performance tests to test the open circuit voltage (VOC), short circuit current (JSC), fill factor (FF) and photoelectric conversion efficiency (PCE) of the perovskite cells. The test results are shown in Table 1.

[0130] Table 1 Test data of embodiments and comparative examples project VOC(V) <![CDATA[JSC(mA / cm 2 )]]> FF(%) PCE(%) Example 1 1.224 19.995 83.125 20.344 Example 2 1.214 19.983 81.365 19.739 Example 3 1.217 19.942 81.589 19.801 Example 4 1.221 19.952 82.179 20.020 Example 5 1.216 19.829 80.794 19.481 Example 6 1.214 19.915 81.159 19.622 Example 7 1.210 19.892 80.034 19.264 Example 8 1.205 19.926 79.978 19.203 Example 9 1.196 19.592 79.893 18.721 Example 10 1.201 19.679 79.993 18.906 Embodiment 11 1.199 19.713 80.012 18.912 Example 12 1.200 19.590 78.135 18.368 Comparative Example 1 1.186 19.293 77.256 17.677 Comparative Example 2 1.185 19.289 76.891 17.575 Comparative Example 3 1.179 19.198 76.541 17.325 Comparative Example 4 1.175 19.201 74.267 16.756 Comparative Example 5 1.172 19.229 77.124 17.381 Comparative Example 6 1.169 19.218 72.145 16.208

[0131] Comparative analysis of the above experimental data shows that:

[0132] 1. Comparing Examples 1 to 11 with Comparative Example 5, the open circuit voltage, short circuit current, fill factor and photoelectric conversion efficiency of Examples 1 to 11 are all higher than those of Comparative Example 5. It can be seen that the present application can greatly improve the performance of the perovskite film and the perovskite battery by introducing a volatile ammonium salt additive during the evaporation of the inorganic salt skeleton layer. And from Examples 1 to 3, it can be seen that the ammonium salt additive is ammonium formate, ammonium chloride or ammonium trifluoroacetate, which can improve the performance of the perovskite battery. Therefore, the additive can be any ammonium salt additive that is volatile when heated.

[0133] 2. Comparing Example 1, Example 4, Example 5, Comparative Example 1 and Comparative Example 2, the open circuit voltage, short circuit current, fill factor and photoelectric conversion efficiency of Example 1, Example 4 and Example 5 are all higher than those of Comparative Example 1 and Comparative Example 2; thus, it can be seen that the evaporation rate of lead iodide is controlled at The evaporation rate of the first evaporation source is controlled at The performance of the perovskite battery can be effectively guaranteed. However, if the evaporation rate of lead iodide is too high or too low, the performance of the perovskite battery will be affected. Therefore, it is preferred to control the evaporation rate of lead iodide to

[0134] 3. Comparing Example 4, Example 6, Example 7, Comparative Example 3, and Comparative Example 4, the open circuit voltage, short circuit current, fill factor, and photoelectric conversion efficiency of Example 4, Example 6, and Example 7 are all higher than those of Comparative Example 3 and Comparative Example 4; it can be seen that the evaporation rate of cesium bromide: the evaporation rate of lead iodide is controlled at (0.3-0.5):1, even if the evaporation rate of the second evaporation source: the evaporation rate of the first evaporation source is (0.3-0.5):1, the performance of the prepared perovskite battery can be effectively guaranteed. However, if the evaporation rate of the second evaporation source (cesium bromide) is too large or too small, it will affect the performance of the perovskite battery. Therefore, it is preferred that the evaporation rate of the second evaporation source: the evaporation rate of the first evaporation source is (0.3-0.5):1.

[0135] 4. Comparing Example 4, Examples 8 to 12, and Comparative Example 6, it can be seen that the open circuit voltage, short circuit current, filling factor, and photoelectric conversion efficiency of Example 4 and Examples 8 to 12 are all higher than those of Comparative Example 6; it can be seen that the evaporation rate of the ammonium salt additive: the evaporation rate of lead iodide is controlled at (0.001 to 0.05): 1, even if the evaporation rate of the third evaporation source: the evaporation rate of the first evaporation source is (0.001 to 0.05): 1, the performance of the prepared perovskite battery can be effectively guaranteed. However, if the evaporation rate of the third evaporation source (ammonium salt additive) is too large or too small, it will affect the performance of the perovskite battery. Therefore, it is preferred that the evaporation rate of the third evaporation source: the evaporation rate of the first evaporation source is (0.001 to 0.05): 1.

[0136] In summary, the preparation method of the perovskite film of the present application introduces a volatile ammonium salt additive during the evaporation process of the inorganic salt skeleton layer, so that the inorganic salt skeleton layer obtained by evaporation contains the ammonium salt additive. During the first annealing process, the ammonium salt additive evaporates and leaves, and forms a number of pores in the inorganic salt skeleton layer during the outward volatilization process, which is conducive to the subsequent penetration and reaction of the organic salt, so that the lead iodide in the inorganic salt skeleton layer reacts thoroughly, and the perovskite nucleus can grow smoothly, which can effectively adjust the film quality of the perovskite film and improve the performance of the perovskite film and the performance of the perovskite battery. In addition, in the first evaporation operation, the evaporation rate of the first evaporation source (lead iodide) is controlled at The evaporation rate of the second evaporation source (cesium bromide): the evaporation rate of the first evaporation source (lead iodide) is (0.3-0.5):1, and the evaporation rate of the third evaporation source (ammonium salt additive): the evaporation rate of the first evaporation source (lead iodide) is (0.001-0.05):1, so as to obtain a perovskite cell with better performance.

[0137] So far, the technical solutions of the present application have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present application is obviously not limited to these specific embodiments. Without departing from the principles of the present application, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present application.

Claims

1. A method for preparing a perovskite film, It is characterized in that The following steps are involved: An inorganic salt skeleton layer containing an additive is prepared on the surface of the substrate by a first evaporation operation, and then a first annealing treatment is performed to obtain an inorganic salt skeleton layer having a plurality of pores inside on the surface of the substrate; An organic layer is prepared on the surface of the inorganic salt skeleton layer having a plurality of pores therein by a second evaporation operation, and then a second annealing treatment is performed to obtain a perovskite film on the surface of the substrate; Wherein, the additive at least includes an ammonium salt additive that can volatilize during the first annealing treatment process.

2. The method for preparing a perovskite thin film according to claim 1, It is characterized in that The ammonium salt additive includes at least one of ammonium formate, ammonium acetate, ammonium chloride and ammonium trifluoroacetate.

3. The method for preparing a perovskite thin film according to claim 1, It is characterized in that The evaporation sources in the first evaporation operation include a first evaporation source, a second evaporation source and a third evaporation source, the first evaporation source includes at least lead iodide, the second evaporation source includes at least one of cesium bromide and cesium iodide, and the third evaporation source includes at least the ammonium salt additive.

4. The method for preparing a perovskite thin film according to claim 3, It is characterized in that In the first evaporation operation, the evaporation rate of the first evaporation source is The evaporation rate of the second evaporation source is (0.3-0.5) : 1; And / or, in the first evaporation operation, the evaporation rate of the first evaporation source is The evaporation rate of the third evaporation source: the evaporation rate of the first evaporation source is (0.001-0.05):

1.

5. The method for preparing a perovskite thin film according to claim 1, It is characterized in that In the first evaporation operation, the evaporation thickness of the inorganic salt skeleton layer is 200 to 310 nm; And / or, in the first annealing process, the annealing temperature is 150-250° C., and the annealing time is 5-30 min.

6. The method for preparing a perovskite thin film according to claim 1, It is characterized in that The evaporation source in the second evaporation operation includes at least one of formamidine iodide, formamidine bromide, formamidine chloride, methylamine iodide, methylamine bromide, and methylamine chloride; And / or, in the second evaporation operation, the evaporation rate of the evaporation source is And / or, in the second evaporation operation, the evaporation thickness of the organic layer is 250-350 nm.

7. The method for preparing a perovskite thin film according to claim 1, It is characterized in that The second annealing process includes a first annealing stage and a second annealing stage performed sequentially, The first annealing stage is specifically annealing in an inert gas atmosphere in a glove box, the annealing temperature is 130-160° C., and the annealing time is 3-20 min; The second annealing stage is performed in air with a humidity RH of 30% to 40%, the annealing temperature is 130 to 150° C., and the annealing time is 10 to 60 minutes.

8. A perovskite film, It is characterized in that The perovskite film is prepared by the method for preparing a perovskite film according to any one of claims 1 to 7.

9. A perovskite battery, It is characterized in that The perovskite cell comprises the perovskite film according to claim 8.

10. A method for preparing a perovskite battery, It is characterized in that The following steps are involved: Preparing a hole transport layer on the conductive side surface of a transparent conductive substrate to obtain a substrate; A perovskite film is prepared on the surface of the hole transport layer by using the method for preparing a perovskite film according to any one of claims 1 to 7; preparing a passivation material layer on the surface of the perovskite film by a third evaporation operation, and then performing a third annealing treatment to obtain a passivation layer; Preparing an electron transport layer on the surface of the passivation layer; preparing a buffer layer on the surface of the electron transport layer; An electrode layer is prepared on the surface of the buffer layer.

11. The method for preparing a perovskite battery according to claim 10, It is characterized in that The hole transport layer includes a first material layer and a second material layer sequentially stacked on the transparent conductive substrate, The material of the first material layer is nickel oxide, The material of the second material layer includes at least one of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid, [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], and 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline.

12. The method for preparing a perovskite battery according to claim 10, It is characterized in that The hole transport layer is prepared by any one of spin coating, slit coating, magnetron sputtering or evaporation; And / or, the hole transport layer has a thickness of 1 to 50 nm.

13. The method for preparing a perovskite battery according to claim 11, It is characterized in that The first material layer is made by magnetron sputtering, and the second material layer is made by spin coating.

14. The method for preparing a perovskite battery according to claim 10, It is characterized in that The evaporation source of the third evaporation operation includes at least one of phenylethylamine iodide, 4-trifluoromethyl-aniline iodide, 2-thiopheneethylamine iodide, ethylamine salt iodide, and guanidine iodide; And / or, in the third evaporation operation, the evaporation rate of the evaporation source is and / or, in the third evaporation operation, the evaporation thickness of the passivation material layer is 1 to 10 nm; And / or, the third annealing treatment is specifically performed in an inert gas atmosphere in a glove box, with an annealing temperature of 60 to 120° C. and an annealing time of 1 to 5 min.

15. The method for preparing a perovskite battery according to claim 10, It is characterized in that The material of the electron transport layer is any one of fullerene and its derivatives; And / or, the material of the buffer layer is one of bathocuproin or atomic layer deposited tin dioxide; And / or, the material of the electrode layer is any one of metal electrode silver, metal electrode copper, transparent conductive oxide ITO, indium zinc oxide, tungsten-doped indium oxide and aluminum-doped zinc oxide.

Citation Information

Cited By

  • Perovskite precursor solution, perovskite solar cell and preparation method thereof

    CN119907612A