Copper alloy powder for laminate forming, method for producing same, method for evaluating same, method for producing copper alloy laminate, and copper

By adding an appropriate amount of magnesium to the copper alloy and carrying out specific aging treatment, the problem of mutual restraint between strength and conductivity in the copper alloy laminated shape is solved, and the manufacturing of high-strength and high-conductivity copper alloy laminated shape is realized. .

CN118984745APending Publication Date: 2024-11-19FUKUDA METAL FOIL & POWDER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094055.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-25
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The strength and conductivity of the existing copper alloys are mutually restricted, and it is difficult to obtain a copper alloy laminated shape with high strength and high conductivity at the same time.

Method used

The copper alloy powder containing chromium or less than 0.70% by weight or less and 1.5% by weight or less and 0.05% by weight or less magnesium or less is produced by lamination forming method, and aging treatment of 400°C or more and 500°C or less is performed. , to improve conductivity and mechanical strength.

Benefits of technology

A copper alloy layered structure with high strength and high conductivity is achieved, meeting the need to simultaneously improve conductivity and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984745A_ABST
    Figure CN118984745A_ABST
Patent Text Reader

Abstract

Provided is a copper alloy powder for laminate molding, with which it is possible to obtain a copper alloy laminate molded body having high strength and high conductivity. The present invention is a copper alloy powder for laminate molding, which is used for molding a laminate molded article by a laminate molding method, and which contains 0.70 wt% to 1.5 wt% (inclusive) of chromium and 0.05 wt% to 0.35 wt% (inclusive) of magnesium, with the remainder comprising copper and unavoidable impurities. Furthermore, the present invention is a method for evaluating a copper alloy powder for laminate molding, the method comprising: a step for performing laminate molding on a copper alloy laminate molding using a copper alloy powder for laminate molding that is to be evaluated; a step for measuring the conductivity X (% IACS) and the Vickers hardness Y (Hv) of the copper alloy laminate; and a step in which, when the conductivity X (% IACS) and the Vickers hardness Y (Hv) are plotted in a two-dimensional chart comprising the X-axis and the Y-axis, the copper alloy powder for laminate molding is evaluated on the basis of whether or not the point (X, Y) is located further toward the high strength side and the high conductivity side than a boundary line represented by (Y =-1.1 X + 300).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copper alloy powder for laminated molding, a method for producing the powder and an evaluation method thereof, a method for producing a copper alloy laminated molded body, and a copper alloy laminated molded body. Background Art

[0002] In the above technical field, Patent Document 1 discloses a copper alloy powder for laminated molding, which is produced by an atomization method and contains more than 1.00 mass % and not more than 2.80 mass % of chromium and the remainder copper.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 6389557 Summary of the invention

[0006] Problems to be solved by the invention

[0007] However, generally, there is a trade-off between the strength (hardness) and electrical conductivity of copper alloys, and the techniques described in the above-mentioned documents cannot produce a copper alloy laminated body having high strength and high electrical conductivity.

[0008] An object of the present invention is to provide a technology for solving the above-mentioned problems.

[0009] Means for solving problems

[0010] In order to achieve the above-mentioned object, the copper alloy powder for laminated molding according to the present invention is a copper alloy powder for laminated molding used for molding a laminated object by a laminated molding method.

[0011] The copper alloy powder for laminated molding contains 0.70 wt % to 1.5 wt % of chromium and 0.05 wt % to 0.35 wt % of magnesium, with the remainder being copper and inevitable impurities.

[0012] In order to achieve the above-mentioned object, the copper alloy laminated body according to the present invention is the following copper alloy laminated body,

[0013] The copper alloy laminated body is obtained by using the above-mentioned copper alloy powder for laminated molding and performing laminated molding using a laminated molding apparatus.

[0014] The copper alloy laminated body contains 0.70 wt% to 1.5 wt% of chromium and 0.05 wt% to 0.35 wt% of magnesium, with the remainder being copper and inevitable impurities.

[0015] In order to achieve the above-mentioned object, the manufacturing method of the copper alloy stacked body according to the present invention comprises the following steps:

[0016] A layered forming step, using the copper alloy powder for layered forming to form a copper alloy layered body by using a layered forming device; and

[0017] In the aging treatment step, the copper alloy laminated body is maintained at a temperature of 400°C to 500°C.

[0018] In order to achieve the above-mentioned object, the present invention relates to a method for producing a copper alloy powder for laminated molding, which is used to form a laminated object by a laminated molding method, and the method comprises the following steps:

[0019] A step of producing a copper alloy powder by a gas atomization method or a plasma rotating electrode method, wherein the copper alloy powder contains 0.70 wt% to 1.5 wt% of chromium and 0.05 wt% to 0.35 wt% of magnesium, with the remainder being copper and unavoidable impurities; and

[0020] A step of classifying the produced copper alloy powder so as to have a particle size of 10 μm to 45 μm, and a particle size of 45 μm to 105 μm.

[0021] In order to achieve the above-mentioned object, the evaluation method of the copper alloy powder for stacking molding according to the present invention comprises the following steps:

[0022] A step of laminating a copper alloy laminated body using the copper alloy powder for laminating as an evaluation object;

[0023] The step of measuring the electrical conductivity X (%IACS) and the Vickers hardness Y (Hv) of the copper alloy laminated body; and

[0024] A process for evaluating the copper alloy powder for laminated molding according to whether the point (X, Y) is located closer to the high strength side and the high conductivity side than the boundary line represented by (Y=-1.1X+300) when the conductivity X (%IACS) and the Vickers hardness Y (Hv) are plotted on a two-dimensional graph consisting of an X-axis and a Y-axis.

[0025] Effects of the Invention

[0026] According to the present invention, a copper alloy laminated body having high strength and high electrical conductivity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] [ Figure 1 ] is a graph showing the relationship between the Vickers hardness and the electrical conductivity of the stacked structure in Patent Document 1 and the boundary line.

[0028] [ Figure 2 ] is a flow chart showing the steps of a method for evaluating copper alloy powder for laminated molding in this embodiment.

[0029] [ Figure 3 ] are binary alloy phase diagrams of copper and magnesium and binary alloy phase diagrams of chromium and magnesium in the copper alloy powder for laminated molding used in this embodiment.

[0030] [ Figure 4 ] is a graph showing the relationship between the Vickers hardness and the electrical conductivity of the copper alloy laminated bodies obtained in this embodiment and the comparative example, as well as the boundary line. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the components described in the following embodiments are merely illustrative, and the technical scope of the present invention is not limited thereto.

[0032] [First embodiment]

[0033] In this embodiment, a new evaluation method of copper alloy powder for laminated molding is described. Prior to this, the current status of copper alloy powder for laminated molding is described.

[0034] <Current Status of Copper Alloy Powder for Laminated Molding>

[0035] The lamination molding technology can produce products with complex shapes that are difficult to produce using conventional processing technologies, and is expected to be used in various fields. In particular, the application of metal materials with excellent mechanical properties is expected.

[0036] Among metal materials, copper has excellent electrical and thermal conductivity, and therefore is expected to be used in products with complex shapes such as normal heat sinks and heat exchangers in laminated molding. However, the materials used as metal powders for laminated molding are mainly iron, nickel, aluminum, titanium, etc. and their alloys, and there are few examples of copper and copper alloys. The reason is that copper has high electrical and thermal conductivity, so when laminated molding is used, the heat energy injected by lasers is quickly dissipated and diffused, and the copper cannot be fully melted, making it difficult to obtain a high-density laminated body.

[0037] In contrast, Patent Document 1 discloses a copper alloy powder for laminated molding, which is manufactured by an atomization method, and contains chromium in an amount of more than 1.00 mass % and less than 2.80 mass % and the remainder of copper. The copper alloy powder is quenched and solidified from a molten state during manufacturing, thereby supersaturated with chromium solid solution, so that thermal diffusion and heat dissipation are reduced, and thermal conductivity is reduced, so that even a low-output molding device can be easily melted and molded. Moreover, during laminated molding, the molding area is temporarily melted and then quenched and solidified, thereby becoming a state of supersaturated with chromium solid solution, so that by performing an aging treatment on the laminated molding, chromium is precipitated from copper as a matrix, and the purity of the copper matrix is ​​increased, the electrical conductivity is improved, and the strength improvement brought about by precipitation strengthening can be achieved at the same time.

[0038] According to the embodiment of Patent Document 1, a copper alloy laminated body having hardness and electrical conductivity of 47.64% IACS to 73.96% IACS and Vickers hardness of 213.3 Hv to 259.8 Hv is obtained by aging treatment at a temperature of 450°C to 500°C where the strength is the highest.

[0039] <Evaluation Method of Copper Alloy Powder for Laminated Forming>

[0040] However, in general, the strength, hardness and electrical conductivity of copper alloys are mutually restrictive. For example, in the case of the laminated structure described in Patent Document 1, the relationship between the Vickers hardness and electrical conductivity during aging treatment at 500°C to 700°C is: Figure 1 so. Figure 1 This is a graph showing the relationship between the Vickers hardness and the electrical conductivity of the laminated structure in Patent Document 1 and the boundary line.

[0041] like Figure 1 As shown in FIG. 1 , the relationship between the Vickers hardness Y (Hv) and the electrical conductivity X (%IACS) is limited to the lower region, that is, the region on the low strength side and the low electrical conductivity side, relative to the boundary line represented by the following formula (1). Including the case of Patent Document 1, the electrical conductivity can usually be improved by increasing the aging treatment temperature or increasing the aging treatment time, but over-aging will occur, the precipitated chromium particles will coarsen, and the strength will be greatly reduced. In other words, this means that under the aging treatment conditions with the highest strength, chromium is not completely precipitated from the copper matrix, and chromium exceeding the solid solubility limit remains in the matrix.

[0042] [Mathematical formula 1]

[0043] Y=-6X+680 (1)

[0044] It is desirable for a practical copper alloy for laminated molding to achieve not only high density and the excellent electrical conductivity inherent in copper, but also higher levels of electrical conductivity and mechanical strength. However, as described above, there is a mutually restrictive relationship between electrical conductivity and strength, and therefore it is not easy to achieve both characteristics at the same time. For example, in Patent Document 1, a copper alloy for laminated molding having a region located above the boundary line represented by the above formula (1), that is, a region on the high strength side and the high electrical conductivity side, is not obtained.

[0045] In this embodiment, from the perspective of achieving both electrical conductivity and mechanical strength at a higher level within the aging treatment range of 400°C to 500°C, equation (2) is used as a reference as a benchmark for specifically expressing high strength and high electrical conductivity. By placing electrical conductivity (% IACS) on the X-axis and Vickers hardness (Hv) on the Y-axis, the characteristics are plotted on a graph, so that the balance between strength and electrical conductivity can be evaluated based on a linear function on the XY graph. Since there is a mutually restrictive relationship between strength and electrical conductivity, the higher the electrical conductivity, the lower the Vickers hardness. Therefore, on the XY graph, it can be represented as a linear function with a negative slope.

[0046] [Mathematical formula 2]

[0047] Y=-1.1X+300 (2)

[0048] In metals, it is known that electrical conductivity and thermal conductivity are in a substantially proportional relationship as per the Wiedemann-Franz law. Therefore, the copper alloy laminated body obtained by laminated molding using the copper alloy powder for laminated molding of the present invention and the laminated molding apparatus has excellent electrical conductivity and can therefore also be used as a copper alloy laminated body having high thermal conductivity.

[0049] (Procedure of Evaluation Method of Copper Alloy Powder for Laminated Forming)

[0050] Figure 2 It is a flowchart showing the procedure of the evaluation method of the copper alloy powder for laminated molding in this embodiment.

[0051] exist Figure 2 In step S201, a powder layer forming process for stacking is performed using the copper alloy powder for stacking molding as the evaluation object. Then, in step S202, it is determined whether a powder layer capable of stacking molding can be formed using the copper alloy powder for stacking molding as the evaluation object. In the case where the squeegeeing property is poor and a powder layer capable of stacking molding cannot be formed, in step S209, it is evaluated as insufficient as the copper alloy powder for stacking molding.

[0052] On the other hand, when the coating property is sufficient to form a powder layer capable of being stacked, in step S203, a stacked body is manufactured using a stacking device or the like using the copper alloy powder for stacking as the evaluation object. In step S204, the electrical conductivity X (% IACS) and the Vickers hardness Y (Hv) of the manufactured stacked body are measured. In step S205, a two-dimensional graph (see FIG. 2 ) with the measured electrical conductivity X (% IACS) and the Vickers hardness Y (Hv) as axes is determined. Figure 4 ) is in the upper area (Y≥-1.1X+300) of the boundary line (Y=-1.1X+300).

[0053] If it is in the upper region (Y≥-1.1X+300), it is evaluated as sufficient as copper alloy powder for laminated molding in step S207. On the other hand, if it is in the lower region (Y<-1.1X+300), it is evaluated as insufficient as copper alloy powder for laminated molding in step S209.

[0054] According to the evaluation method of the copper alloy powder for layered molding of the present embodiment, it is possible to evaluate the copper alloy powder for layered molding that can obtain a copper alloy layered molding having high strength and high electrical conductivity.

[0055] [Second embodiment]

[0056] In the present embodiment, the characteristics of the copper alloy powder for laminated molding that obtains a sufficiently satisfactory result in the evaluation method of the copper alloy powder for laminated molding according to the first embodiment will be described.

[0057] <For highly rated materials>

[0058] In this embodiment, a method for producing a raw material powder capable of achieving characteristics in a region above the boundary line represented by the above formula (2), that is, a region on the high strength side and the high conductivity side, as well as the raw material powder and a laminated body obtained using the raw material powder are provided.

[0059] The inventors of the present application targeted the region above the boundary line represented by the above formula (2), that is, the region on the high strength side and the high conductivity side. As a result, by setting it as a ternary alloy in which magnesium is added to a copper-chromium alloy, an alloy having the characteristics of the region above the boundary line represented by the above formula (2), that is, the region on the high strength side and the high conductivity side was discovered.

[0060] That is, in order to achieve high electrical conductivity and high mechanical strength at a high level with good balance, chromium needs to be fully and completely precipitated even at a relatively low aging treatment temperature. In order to promote the precipitation of solute elements from the solvent elements serving as the matrix, it is effective to increase the chemical potential of the solute elements. Therefore, it is believed that if an element that increases the chemical potential of chromium in the matrix is ​​added to the copper-chromium alloy, the mutual repulsion between the elements will increase, the chemical potential of chromium will increase, and the precipitation of chromium can be promoted. Therefore, the addition of an element that increases the chemical potential of chromium as a third element to the copper-chromium alloy was studied. A search was conducted among various elements for a candidate for a third element with a high mutual repulsion, and magnesium was discovered. From Figure 3 It can be inferred from the phase diagram that magnesium is likely to have a high mutual repulsion with both chromium and copper as the matrix, so it is believed that even a small amount of magnesium can effectively act on the increase of the chemical potential of chromium. In addition, even among the alloying elements for copper, magnesium is one of the elements that has the least effect on increasing the resistivity of the matrix, and it can be expected that even if it is added to the copper-chromium alloy as a third element, the influence on the conductivity can be suppressed to a minimum. Based on the above, the inventors of the present application thought of adding magnesium as a third element to the copper-chromium alloy, and conducted intensive research to complete the present invention.

[0061] Based on the above-mentioned studies, in the present embodiment, a copper alloy powder for laminated molding and a laminated molded body thereof can be provided, which can achieve both high electrical conductivity and high strength at high levels.

[0062] More specifically, the copper alloy powder for laminated molding according to the present embodiment contains 0.70 wt% to 1.5 wt% of chromium and 0.05 wt% to 0.35 wt% of magnesium, with the remainder being copper and inevitable impurities.

[0063] In addition, the 50% particle size of the copper alloy powder for laminated molding according to the present embodiment is 3.0 μm or more and 200 μm or less.

[0064] In addition, the apparent density of the copper alloy powder for laminated molding of the present embodiment when measured by the measuring method of JIS Z 2504 is 3.5 g / cm 3 above.

[0065] In addition, regarding the copper alloy powder for laminated molding according to the present embodiment, the adhesion of the copper alloy powder obtained from the fracture envelope obtained by the shear test is 0.600 kPa or less.

[0066] The copper alloy stacked molded body of the present embodiment is formed by stacking using the copper alloy powder for stacking molding of the present embodiment and using a stacking molding device, and contains 0.70 weight % to 1.5 weight % of chromium and 0.05 weight % to 0.35 weight % of magnesium, with the remainder consisting of copper and unavoidable impurities.

[0067] The copper alloy laminated structure of the present embodiment has an electrical conductivity of 60% IACS or more.

[0068] The copper alloy laminated body of the present embodiment has a Vickers hardness of 230 Hv or more.

[0069] The method for producing the copper alloy laminated body of the present embodiment further includes an aging treatment step of holding the copper alloy laminated body of the present embodiment at 400 to 500° C., more preferably 450 to 500° C.

[0070] For the copper alloy powder for stacked molding of the present embodiment, by adding magnesium as the third element to the copper-chromium alloy, it is possible to produce a copper alloy stacked molded body having excellent electrical conductivity and mechanical strength in a region located above the boundary line represented by the above formula (2), that is, a region on the high strength side and the high electrical conductivity side.

[0071] (Copper Alloy Powder for Laminated Forming of the Present Embodiment)

[0072] The manufacturing method of the copper alloy powder for stacking molding of the present embodiment is not particularly limited, and preferably a method in which the powder particles are quenched and solidified from a molten state such as gas atomization, water atomization, centrifugal atomization, plasma atomization, plasma rotating electrode method, etc. is used. From the perspective of mass production, gas atomization is particularly preferred. The manufactured powder can be classified under prescribed classification conditions using a known classification method to adjust the copper alloy powder for stacking molding to an appropriate particle size. As a classification device for implementing classification, an air flow classifier can be preferably used.

[0073] In the copper-chromium alloy as a precipitation-strengthened copper alloy, chromium supersaturated in the copper as the matrix is ​​precipitated by aging treatment, and the strength of the copper alloy is improved. In order to obtain a copper alloy laminated body with high mechanical strength, the chromium content is preferably 0.70% by weight or more. In the case of less than 0.70% by weight, the precipitation amount in the aging treatment becomes insufficient, and the effect of improving strength cannot be fully obtained. The solid solubility limit of chromium relative to copper is said to be 0.7% by weight or more and 0.8% by weight or less at the eutectic temperature of about 1076°C. Although the amount is small, when a method such as atomization is used to melt the metal and rapidly solidify it as a powder manufacturing method, chromium above the solid solubility limit can be included in the copper matrix. In addition, in the case of a laminated body forming method using a powder bed melting method, from the perspective of its process, melting and rapid solidification based on a laser or electron beam are performed, so that a laminated body can be made in a state where chromium above the solid solubility limit is contained in the copper matrix. However, when the chromium content exceeds 1.5 wt%, the mechanical strength can be further improved, but the electrical conductivity is greatly reduced. Therefore, the chromium content is preferably 1.5 wt% or less.

[0074] As mentioned above, magnesium is an important element that is considered to increase the chemical potential of chromium, enhance the mutual repulsion between elements and promote the precipitation of chromium. When the magnesium content is less than 0.05% by weight, the precipitation of chromium becomes insufficient, and it is impossible to simultaneously meet the high strength and high conductivity of the present invention with good balance. When the magnesium content is greater than 0.35% by weight, the ratio of magnesium increases, but even if magnesium is increased, no significant effect is obtained in terms of characteristics. In addition, due to the excessive inclusion of expensive magnesium, an increase in cost is caused. Therefore, the magnesium content is preferably set to more than 0.05% by weight and less than 0.35% by weight, and more preferably set to more than 0.06% by weight and less than 0.25% by weight.

[0075] It should be noted that the copper alloy powder for laminated molding of the present embodiment may contain inevitable impurities in addition to chromium and magnesium. Inevitable impurities are substances that are inevitably mixed in the manufacturing process of the copper alloy powder for laminated molding, and examples thereof include oxygen, phosphorus, iron, aluminum, silicon, titanium, etc. These inevitable impurities may reduce the electrical conductivity, and therefore, are preferably set to 0.10 wt% or less, more preferably set to 0.05 wt% or less, and even more preferably set to 0.01 wt% or less.

[0076] The powder used for layered molding is required to be suitable for the various processes of layered molding, such as the process of supplying from the feed hopper to the molding table, the process of forming a powder layer evenly spread with a certain thickness, and the process of melting and solidification. Therefore, the following conditions are required. The conditions refer to: the particle size adjusted to an appropriate range, the apparent density within an appropriate range, and the fluidity of the powder that can be supplied from the feed hopper and form an appropriate powder layer.

[0077] The 50% particle size of the copper alloy powder for stacking molding is the cumulative value 50% particle size of the powder in the cumulative particle size distribution based on volume when measured by laser diffraction method (the so-called median particle size, D50), and is preferably included in the range of 3.0μm to 200μm. When the 50% particle size is less than 3.0μm, the fluidity of the powder does not exist, and a powder bed cannot be formed even in a stacking molding device of the laser powder bed melting method. In addition, the powder is violently scattered and reattached to the stacking molding body, etc., resulting in surface defects. When the 50% particle size is greater than 100μm when stacking molding is performed by laser powder bed melting method, and when the 50% particle size is greater than 200μm when stacking molding is performed by electron beam powder bed melting method, the surface of the powder bed is rough and a powder bed suitable for molding cannot be formed. In addition, the surface of the stacked shape becomes rough, resulting in poor appearance. When the light beam is irradiated, the molten pool generated in the powder layer does not reach the solidification layer directly below, resulting in insufficient melting and solidification, which will cause poor shaping. In the laser powder bed fusion method, the 50% particle size is preferably 3.0 μm to 100 μm, more preferably 5.0 μm to 75 μm, and even more preferably 10 μm to 45 μm. In the electron beam powder bed fusion method, the 50% particle size is preferably 10 μm to 200 μm, more preferably 25 μm to 150 μm, and even more preferably 45 μm to 105 μm.

[0078] The apparent density of the copper alloy powder for laminated molding is preferably 3.5 g / cm 3 Above. The apparent density is less than 3.5g / cm 3 In the case of the powder filling rate of the powder layer filled by brushing is reduced, and an appropriate powder layer cannot be formed. In addition, since the filling property of the powder is reduced, voids are generated in the stacked shape, and the density of the stacked shape is reduced.

[0079] In the layered molding method, fluidity is a particularly important powder property. In particular, in the powder bed fusion method, it is the most important powder property directly related to the quality of the layered molding body in the powder supply from the feed hopper and the powder supply from the coater, and the formation of the powder layer on the molding table. In the powder bed fusion method, the powder needs to be evenly spread on the molding table with a certain thickness. The process of spreading the powder is called brushing, and the quality of the powder spreading is called brushing property. The powder used in the layered molding method needs sufficient brushing property, so the powder needs appropriate fluidity. As an indicator for measuring the fluidity of metal powder, the fluidity (FR: Flow Rate) specified in JIS Z 2502 "Metal Powder-Flowability Determination Method" can be used, but in the fine powder with a 50% particle size of less than 50μm mainly used for the laser powder bed fusion method, sometimes the powder does not flow out of the measurement container and cannot be measured, and the fluidity cannot be evaluated. Therefore, as an index for evaluating the fluidity of fine powder, it is effective to use the adhesion of powder obtained by the direct shear test method of powder (hereinafter referred to as shear test) specified in the "direct shear test method of powder" of the Japan Powder Industry Technology Association Standard (SAP15-13: 2013). For adhesion, in the shear test, the shear stress generated when the powder layer formed by compacting in the vertical direction is pressed in the vertical direction is measured to make it slide laterally in the horizontal direction, thereby being able to be obtained from the failure envelope of the obtained powder layer. In the shear test, it can be measured by using, for example, a powder rheometer FT4 manufactured by Freeman Technology. For copper alloy powder for stacking molding, if its adhesion is less than 0.600 kPa, it can be judged that it has sufficient fluidity to spread a uniform powder layer and has good brushability. Thus, a high-density and homogeneous stacked body can be obtained. In the case where the adhesion is greater than 0.600 kPa, the fluidity of the copper alloy powder for stacking molding is insufficient, the brushability becomes poor, and an appropriate powder layer cannot be formed. Therefore, in the copper alloy powder for laminated molding, it is desired that the adhesion of the copper alloy powder obtained from the fracture envelope obtained by a shear test is 0.600 kPa or less.

[0080] (Copper Alloy Laminated Body of the Present Embodiment)

[0081] In order to produce copper alloy laminated bodies, various known metal laminated forming technologies can be used. For example, in the powder bed melting method, the laminated body is produced while repeatedly performing the following steps: using a scraper or roller to level and spread the metal powder on the forming table to form a powder layer, irradiating the specified position of the formed powder layer with a laser or electron beam to sinter and melt the metal powder. In the forming process of metal laminated forming, in order to obtain high-quality laminated bodies, it is necessary to control a lot of process parameters. In the laser powder bed melting method, there are many scanning conditions such as laser output power and laser scanning speed. Therefore, when setting the optimal scanning conditions, the energy density, which is an index summarizing the main parameters, is used to adjust the main parameters. If the output power of the laser is set to P [W], the scanning speed of the laser is set to v [mm / s], the laser scanning interval is set to s [mm], and the thickness of the powder layer is set to t [mm], then the energy density E [J / mm 3 ] is determined by E = P / (v×s×t). In the laser powder bed fusion method, the energy density is preferably 150 J / mm 3 Above 450J / mm 3 Below. When the energy density is less than 150J / mm 3 In the case of high energy density, the powder layer may not be melted or fused properly, and voids may be formed in the laminated body. 3 In the case of sputtering, the surface of the powder layer becomes unstable, and defects such as voids are generated in the stacked body. In the electron beam powder bed melting method, when the electron beam is irradiated to the powder layer, if negative charges are accumulated in the powder layer and charged, it will cause a smoke phenomenon in which the powder flies in a mist-like manner, resulting in poor melting. Therefore, in order to prevent charging, a preparatory process is required to preheat the powder layer and temporarily sinter it. However, when the preheating temperature is too high, sintering progresses and causes necking, and it is difficult to remove the remaining powder from the inside of the stacked body after forming. Therefore, in the copper alloy powder for stacking forming, the preheating temperature is preferably set to 400 to 800°C. It should be noted that the metal stacking forming technology based on the powder bed melting method is exemplified here, but as a general stacking forming method for making a stacked body using the copper alloy powder for stacking forming of the present invention, it is not limited to this. For example, a stacking forming method based on a directional energy deposition method can also be used.

[0082] (Aging treatment)

[0083] By subjecting the stacked body to aging treatment, the supersaturated solid solution of chromium is precipitated, the strength of the stacked body is improved, and the electrical conductivity is improved. Therefore, the aging treatment process is a necessary process for obtaining the high strength and high electrical conductivity characteristics of the present invention. The aging treatment can be implemented by heating the stacked body to a specified temperature and maintaining it for a specified time. The aging treatment is preferably carried out in a reducing atmosphere or an inert gas in a vacuum. The effect of the aging treatment is determined by the combination of the aging treatment temperature and the aging treatment time. Therefore, in terms of balancing the target characteristics and efficiency, it is important to set appropriate conditions. The aging treatment temperature is preferably above 400°C and below 500°C. More preferably, it is above 450°C and below 500°C. In the case where the mechanical strength is particularly improved, it is preferably set to 450°C. In the case where a particularly high electrical conductivity is desired, it can also be set to above 500°C. When the aging treatment temperature is lower than 500°C, the aging treatment time is preferably set to be more than 0.5 hours and less than 10 hours. When the aging treatment temperature is higher than 500°C, the aging treatment time is preferably set to be more than 0.5 hours and less than 3 hours. When the aging treatment time is less than the above-mentioned set time, the precipitation of chromium becomes insufficient. In addition, when the aging treatment temperature exceeds the above-mentioned set time, it becomes over-aging, and the precipitated chromium coarsens, resulting in a decrease in hardness. When the aging treatment temperature is lower than 400°C, it takes a long time until the aging effect is obtained, which is not practical. In addition, when the aging treatment temperature exceeds 500°C, it becomes over-aging, the precipitated chromium phase coarsens and the strength decreases. In the laminated body made using the copper alloy powder for laminated forming of the present invention, due to the mutual repulsion between chromium and magnesium, even if the aging treatment temperature is 450°C and the aging treatment time is about several hours, the electrical conductivity and mechanical strength can be fully improved.

[0084] (Evaluation of Copper Alloy Laminated Structures)

[0085] The Vickers hardness is measured by a method in accordance with “JIS Z 2244: Vickers hardness test-test method.” The Vickers hardness can be measured, for example, using a micro hardness tester HMV-G21-DT manufactured by Shimadzu Corporation.

[0086] The laminated body has an electrical conductivity of 60% IACS or more. The electrical conductivity can be measured by, for example, an eddy current conductivity meter. Examples of eddy current conductivity meters include the high-performance eddy current conductivity meter SigmaCheck manufactured by Nihon Matech Corporation. It should be noted that IACS (International Annealed Copper Standard) refers to the standard annealed copper (volume resistivity: 1.7241×10 -2 The electrical conductivity of 100 μΩm) is defined as 100% IACS. The electrical conductivity can be adjusted by aging treatment, and is preferably adjusted appropriately in accordance with the balance between the desired Vickers hardness. The electrical conductivity is preferably 60% IACS or more.

[0087] According to the present embodiment, it is possible to provide a copper alloy powder for laminated molding capable of obtaining a copper alloy laminated body having high strength and high electrical conductivity, and the copper alloy laminated body.

[0088] [Other embodiments]

[0089] The present invention has been described above with reference to the embodiments, but the present invention is not limited to the above embodiments. Various changes that can be understood by those skilled in the art can be made to the configuration and details of the present invention within the technical scope of the present invention.

[0090] Example

[0091] The present invention will be described in detail below based on Examples and Comparative Examples. The following Examples and Comparative Examples are merely specific examples for making the technical content of the present invention easier to understand, and the technical scope of the present invention is not limited by these specific examples.

[0092] Copper alloy powders for stacking molding of various compositions shown in the following Table 1 are manufactured by gas atomization method, and the various copper alloy powders obtained are classified so that the particle size is 10 μm to 45 μm for laser powder bed melting method, and the particle size is 45 μm to 105 μm for electron beam powder bed melting method.

[0093] The contents of the component elements in the obtained copper alloy powder for laminated molding were measured by ICP emission spectrometry. In addition, the apparent density (AD) (g / cm 3) was measured. In addition, the fluidity (FR) (seconds / 50 g) of the obtained copper alloy powder for laminated molding was measured in accordance with JIS Z 2502. In addition, the 50% particle size (D50) (μm) was measured by laser diffraction method (Microtrac MT3300: manufactured by Microtrac BEL Co., Ltd.).

[0094] A shear test was carried out using a powder rheometer FT4 (manufactured by Freeman Technology), and the adhesion (kPa) of the obtained copper alloy powder for stacking molding was measured. The powder for the molding test was actually spread on the molding table of the 3D powder additive manufacturing apparatus (powder bed melting method / laser method or electron beam method) to form a powder layer, and the brushability of the obtained copper alloy powder for stacking molding was evaluated. Regarding the copper alloy powder for stacking molding used in Examples 1 to 4 and Comparative Examples 1 to 10, the measurement results of various powder properties are shown in Table 1. Here, Comparative Example 8 is a copper fine powder for conductive materials using a high-pressure water atomization method, and Comparative Example 9 is a copper spherical powder using a plasma rotating electrode method. The copper alloy powders of Comparative Examples 8 to 10 have poor brushability, so they cannot be brushed and stacking molding cannot be implemented.

[0095] [Table 1]

[0096] Table 1 Powder properties

[0097]

[0098] The copper alloy powder for layered molding in the above-mentioned Examples 1 to 4 and Comparative Examples 1 to 7 was used to produce a layered molding body for testing using a 3D powder layered molding machine (SLM Solutions GmbH, SLM280HL) equipped with a Yb fiber laser with a wavelength of 1064 nm. The layered molding was performed at a layer thickness of 25 μm to 50 μm, a laser output power of 300 W to 700 W, a scanning speed of 900 mm / s to 1500 mm / s, and an energy density of 150 J / mm 3 Above 450J / mm 3 The following conditions were used.

[0099] Use the above-mentioned 3D powder stacking machine to make The height of the laminated body is 10 mm. The density of the laminated body was measured by the Archimedean method using helium as the replacement medium (AccuPyc1330: manufactured by Shimadzu Corporation), and the theoretical density (density of the molten material having the same composition as the laminated body) was set to 100% to calculate the relative density (%). The measurement results are shown in Table 1. It should be noted that the laminated bodies obtained using the copper alloy powder for laminated forming of Comparative Examples 8 to 10 were excluded from the following evaluation of the characteristics of the laminated bodies.

[0100] For the laminated bodies of Examples 1 to 4 and Comparative Examples 1 to 7 manufactured using the 3D powder lamination molding machine, the electrical conductivity (% IACS) was measured using an eddy current conductivity meter (high performance eddy current conductivity meter SigmaCheck: manufactured by Nihon Matech Corporation). In addition, the Vickers hardness (Hv) of each laminated body was measured using a micro hardness tester (micro hardness tester HMV-G21-DT: manufactured by Shimadzu Corporation).

[0101] In an inert atmosphere, the temperature was set to 400°C, 450°C, and 500°C, and the laminated bodies were subjected to aging treatment for 1 hour. The conductivity of the laminated bodies subjected to aging treatment was measured using an eddy current conductivity meter. In addition, the Vickers hardness was measured using a micro hardness tester. The evaluation results of various properties of the laminated bodies of Examples 1 to 4 and Comparative Examples 1 to 7 manufactured using a 3D powder laminated molding machine are shown in Table 2.

[0102] [Table 2]

[0103] Table 2 Characteristics of the shape

[0104]

[0105] Then, based on the evaluation results of various characteristics in Table 2, generate Figure 1 Same Figure 4 . Figure 4 The graph is a graph showing the relationship between the Vickers hardness and the electrical conductivity of the copper alloy laminated bodies obtained in the present embodiment and the comparative example and the boundary line. Figure 4In the examples 1-1 and 1-1, the copper alloy laminated bodies obtained by aging at 400°C using the copper alloy powder for laminated molding of the examples 1 and 1 and the comparative examples 1 are plotted. In addition, the copper alloy laminated bodies obtained by aging at 450°C using the copper alloy powder for laminated molding of the examples 1 and 1 and the comparative examples 1-2 are plotted. Moreover, the copper alloy laminated bodies obtained by aging at 500°C using the copper alloy powder for laminated molding of the examples 1 and 1 and the comparative examples 1-3 are plotted. Hereinafter, the copper alloy powder for laminated molding is evaluated based on whether a copper alloy laminated body having high strength (Vickers hardness of 230 Hv or more) and high electrical conductivity (electrical conductivity of 60% IACS or more) is obtained. It should be noted that, depending on the application of the copper alloy multilayer structure, a copper alloy multilayer structure that does not have high strength and high electrical conductivity may be used.

[0106] (Evaluation of Examples and Comparative Examples)

[0107] In Comparative Examples 1 and 2, since the copper-chromium alloy does not contain magnesium, the high strength and high conductivity of the present invention cannot be satisfied at the same time with good balance. In Comparative Example 3, since the magnesium content is higher than the content of the present invention, the high strength and high conductivity of the present invention cannot be satisfied at the same time with good balance. In Comparative Example 4, since the magnesium content is lower than the content of the present invention, the high strength and high conductivity of the present invention cannot be satisfied at the same time with good balance.

[0108] In addition, although Comparative Example 5 contains magnesium within the range of the present invention, it contains 2.00 wt% of chromium which exceeds the range of the present invention. Therefore, although it shows a high Vickers hardness, the electrical conductivity is low, and it is not possible to simultaneously satisfy the high strength and high electrical conductivity of the present invention in a good balance. Although Comparative Examples 6 and 7 contain magnesium within the range of the present invention, they do not contain a sufficient amount of chromium. Therefore, although the electrical conductivity is sufficient, the strength is insufficient, and it is not possible to simultaneously satisfy the high strength and high electrical conductivity of the present invention in a good balance.

[0109] On the other hand, in Examples 1 to 4, high strength and high electrical conductivity were achieved at the same time with good balance.

[0110] Based on the above, according to the present example, it was confirmed that a copper alloy powder for laminated molding capable of achieving excellent electrical conductivity and strength and a copper alloy laminated molded body excellent in electrical conductivity and strength can be provided.

Claims

1. A copper alloy powder for laminated molding, the copper alloy powder being used for molding a laminated object by a laminated molding method, The copper alloy powder for laminated molding contains 0.70 wt % to 1.5 wt % of chromium and 0.05 wt % to 0.35 wt % of magnesium, with the remainder being copper and inevitable impurities.

2. The copper alloy powder for laminated molding according to claim 1, wherein The copper alloy powder for laminated molding contains 0.70 wt % to 1.5 wt % of chromium and 0.06 wt % to 0.25 wt % of magnesium, with the remainder being copper and inevitable impurities.

3. The copper alloy powder for laminated molding according to claim 1 or 2, wherein a 50% particle size thereof is 3.0 μm or more and 200 μm or less.

4. The copper alloy powder for laminated molding according to any one of claims 1 to 3, wherein The apparent density of the powder when measured by the measurement method of JIS Z 2504 is 3.5 g / cm 3 above.

5. The copper alloy powder for laminated molding according to any one of claims 1 to 4, wherein The adhesion of the copper alloy powder obtained from the fracture envelope obtained by the shear test was 0.600 kPa or less.

6. A copper alloy laminated body obtained by laminating and molding the copper alloy powder for laminating molding according to any one of claims 1 to 5 using a laminating and molding apparatus, The copper alloy laminated body contains 0.70 wt% to 1.5 wt% of chromium and 0.05 wt% to 0.35 wt% of magnesium, with the remainder being copper and inevitable impurities.

7. The copper alloy laminated body according to claim 6, which has an electrical conductivity of 60% IACS or more.

8. The copper alloy laminated body according to claim 7, having a Vickers hardness of 230 Hv or more.

9. A method for manufacturing a copper alloy laminated body, comprising the following steps: a layered forming step, using the copper alloy powder for layered forming according to any one of claims 1 to 5, and performing layered forming of a copper alloy layered body using a layered forming apparatus; and In the aging treatment step, the copper alloy laminated body is maintained at a temperature of 400° C. to 500° C.

10. A method for producing copper powder for laminated molding, the method comprising the following steps: A step of producing a copper alloy powder by a gas atomization method or a plasma rotating electrode method, wherein the copper alloy powder contains 0.70 wt% to 1.5 wt% of chromium and 0.05 wt% to 0.35 wt% of magnesium, with the remainder being copper and unavoidable impurities; and A step of classifying the produced copper alloy powder so as to have a particle size of 10 μm to 45 μm, and a particle size of 45 μm to 105 μm.

11. A method for evaluating a copper alloy powder for laminated molding, the method comprising the following steps: A step of laminating a copper alloy laminated body using the copper alloy powder for laminating as an evaluation object; The step of measuring the electrical conductivity X (%IACS) and the Vickers hardness Y (Hv) of the copper alloy laminated body; and A process for evaluating the copper alloy powder for laminated molding according to whether the point (X, Y) is located closer to the high strength side and the high conductivity side than the boundary line represented by (Y=-1.1X+300) when the conductivity X (%IACS) and the Vickers hardness Y (Hv) are plotted on a two-dimensional graph consisting of an X-axis and a Y-axis.