Aluminum powder product for metal laminate molding and method for manufacturing

By adjusting the ratio of magnesium to oxygen in aluminum powder and sintering under specific conditions, the poor sintering property caused by oxidation of the film on the surface of aluminum powder is solved, and a high-density and high thermal conductivity aluminum powder molding is achieved, which improves manufacturing performance.

CN118984748APending Publication Date: 2024-11-19MITSUBISHI MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028319.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-10
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When using adhesive spraying to manufacture aluminum or aluminum alloy moldings, the oxidized film on the surface of the aluminum powder leads to poor sintering properties, and the light powder is easily scattered during the spraying process, resulting in a decrease in uniformity and filling density, affecting thermal conductivity.

Method used

By adjusting the ratio of magnesium (Mg) to oxygen in the aluminum powder to be 0.1 or more and 2.0 or less, and performing a degreasing step in an oxidation environment of 500°C or heating and sintering in a non-oxidizing gas stream of 1 Pa or more and 100 kPa or less, and heating and sintering are performed in a non-oxidizing gas stream of 1 Pa or more and 100 kPa or less, and , the oxidized film on the surface of the aluminum powder is reduced by an appropriate amount of Mg, so as to improve the sintering property and prevent the thermal conductivity from decreasing.

Benefits of technology

A high-density aluminum sintered body with a relative density of more than 90% is achieved, which improves the sintering and thermal conductivity of aluminum powder moldings, reduces internal defects, and improves the performance of heat exchange parts and conductive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984748A_ABST
    Figure CN118984748A_ABST
Patent Text Reader

Abstract

In this aluminum powder product for metal laminate molding, the purity of aluminum in the entire powder is 98 mass% or more, Mg is contained in an amount of 0.01-0.5 mass%, and the ratio of the contained Mg amount (mass%) to the oxygen amount (mass%), i.e., Mg amount / oxygen amount, is 0.1-2.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum powder product for metal stacking molding and a method for manufacturing an aluminum powder molded object.

[0002] This application claims priority based on patent application No. 2022-048834 filed in Japan on March 24, 2022, and the contents are incorporated herein by reference. Background Art

[0003] Aluminum is widely used as a heat sink material due to its light weight and high thermal conductivity. However, in order to further improve the heat dissipation characteristics, it is required to design and manufacture complex-shaped pins, fins, grids, etc. that can perform more efficient heat exchange. As a method for manufacturing complex-shaped products, metal 3D printers are being used.

[0004] In recent years, the binder jetting method has attracted attention as one of the layered modeling technologies using metal powder. In the binder jetting method, a binder containing a thermosetting resin, a thermoplastic resin or a photocurable resin is selectively sprayed from a print head onto a metal powder layer, and the layers are repeatedly stacked. The following method is known: after obtaining a metal powder molded body fixed to a desired three-dimensional shape through repeated stacking, a three-dimensional metal molded object is obtained through the steps of binder fixing, removal of unnecessary powder, degreasing, and sintering.

[0005] For example, the following Patent Documents 1 and 2 disclose metal lamination molding or molding apparatus thereof using a binder jetting method.

[0006] Patent Document 1: Japanese Patent Application No. 2020-511593

[0007] Patent Document 2: Japanese Patent Application Publication No. 2020-152001

[0008] Patent Document 3: Japanese Patent Application Publication No. 2004-308004

[0009] On the other hand, when a shaped object of aluminum or aluminum alloy is obtained by using a binder spraying method, it is necessary to improve the sintering difficulty caused by the oxide film on the surface of the aluminum powder.

[0010] For example, Patent Document 3 describes a method of using fine powders with a large specific surface area to improve the sinterability of aluminum. However, when applied to a binder spraying method, aluminum with a relatively low specific gravity may scatter when a powder layer is formed, causing a decrease in uniformity or a decrease in filling density, or there may be problems with safety.

[0011] Therefore, when a shaped object of aluminum or aluminum alloy is obtained by using a binder jetting method, it is important to obtain sufficient sinterability while ensuring the fluidity of the metal powder. Summary of the invention

[0012] The present invention is proposed in view of the above-mentioned problems, and its purpose is to provide an aluminum powder product for metal stacking molding and a method for manufacturing an aluminum powder molded object using the aluminum powder product for metal stacking molding. In the aluminum powder product for metal stacking molding, even aluminum powder having an oxide film and known as a difficult-to-sinter material can be applied to the binder injection method.

[0013] Based on the above background, the inventors have studied the use of the following raw materials for binder spraying: the ratio of the amount of magnesium (mass %) to the amount of oxygen (mass %) contained in the aluminum powder as the raw material is adjusted to be greater than 0.1 and less than 2.0, and the amount of oxygen contained in the aluminum powder is less than 0.3 mass %.

[0014] As a result, it was found that a technology was developed that could obtain a high-density aluminum sintered body with a relative density of more than 90% of the true density of the aluminum powder serving as the raw material by carrying out a degreasing process after molding based on a binder injection method at a temperature below 500°C in an oxidizing environment, or by heating and sintering the obtained degreased body in a non-oxidizing gas flow under a reduced pressure of more than 1 Pa and less than 100 kPa.

[0015] Therefore, the present inventors have conducted various studies and, as a result, provide an aluminum powder product for metal laminate molding and a method for producing an aluminum powder molded object using the aluminum powder product for metal laminate molding.

[0016] (Mode 1) The aluminum powder product for metal laminate molding of Mode 1 involved in the present invention is characterized in that the purity of aluminum in the entire powder is 98 mass% or more, it contains Mg in an amount of 0.01 mass% or more and 0.5 mass% or less, and the ratio of the amount of Mg (mass %) to the amount of oxygen (mass %), i.e., Mg amount / oxygen amount, is 0.1 or more and 2.0 or less.

[0017] The aluminum powder product for metal laminated modeling contains an appropriate amount of Mg and has an appropriate amount of oxygen corresponding to the contained Mg. By including an appropriate amount of Mg in the aluminum powder, Mg reduces the oxide film on the particle surface of the aluminum powder product for metal laminated modeling and locally destroys it, thereby improving sinterability. In addition, in order to achieve the reduction reaction on the particle surface of the aluminum powder product for metal laminated modeling, an Mg amount of a certain value or more relative to the oxygen amount is required. In the case of a small amount of Mg, the local destruction of the oxide film on the particle surface of the aluminum powder product for metal laminated modeling cannot be achieved. In the case of an excessive amount of Mg, the sinterability improvement effect caused by the destruction of the oxide film becomes less, thereby causing a decrease in electrical conductivity and a decrease in thermal conductivity caused by an increase in the amount of Mg. The Mg amount is more preferably 0.015 mass% or more and 0.4 mass% or less, and more preferably 0.02 mass% or more and 0.3 mass% or less. The same method can also be used in the following methods 2 to 10.

[0018] In order to achieve the reduction reaction of the surface of the aluminum powder product for metal stacking molding, and to make the sintering property good and prevent the decrease of thermal conductivity, the value of Mg amount / oxygen amount is required to be 0.1 or more and 2.0 or less. The value of Mg amount / oxygen amount can be more preferably 0.015 or more and 0.15 or less, and can be more preferably 0.02 or more and 0.1 or less. The same can also be applied to the following modes 2 to 10.

[0019] (Mode 2) The aluminum powder product for metal laminate molding of Mode 2 preferably contains 0.1 mass % or more and 1.0 mass % or less of Si in addition to the above-mentioned Mg in Mode 1.

[0020] If the Si content is within the above range, it helps to lower the melting point of the aluminum powder product for metal stacking molding, improve sinterability, and maintain high thermal conductivity while suppressing the decrease in electrical conductivity. The Si content can be 0.15 mass% or more and 0.8 mass% or less, and can be more preferably 0.2 mass% or more and 0.7 mass% or less. The same can also be applied to the following modes 3 to 10.

[0021] (Mode 3) The aluminum powder product for metal stacking molding of Mode 3 is characterized in that the aluminum powder product for metal stacking molding is a mixture of aluminum powder with a purity of 99% or more and aluminum alloy powder containing 0.1 mass % or more and 1.0 mass % or less of Mg and 3.0 mass % or more and 12.0 mass % or less of Si, and the ratio of Mg amount (mass %) to oxygen amount (mass %), i.e., Mg amount / oxygen amount, is 0.1 or more and 2.0 or less.

[0022] If it is the aluminum powder product for metal laminate molding as mentioned above, it is possible to contain an appropriate amount of Mg in the entire mixture and have an appropriate amount of oxygen corresponding to the contained Mg. By including an appropriate amount of Mg in the powder mixture, Mg reduces the oxide film on the particle surface of aluminum powder with a purity of 99% or more and locally destroys it, thereby improving sintering properties. In addition, in order to achieve the reduction reaction on the particle surface of aluminum powder or the particle surface of aluminum alloy powder, an amount of Mg that is greater than a certain value relative to the amount of oxygen is required. When the amount of Mg is small, it becomes impossible to achieve local destruction of the oxide film on the particle surface of aluminum powder or the particle surface of aluminum alloy powder. When the amount of Mg is too much, the sintering property improvement effect caused by the destruction of the oxide film becomes less, resulting in a decrease in electrical conductivity and a decrease in thermal conductivity due to the increase in the amount of Mg.

[0023] In the aluminum powder product for metal laminate molding of method 3, in order to achieve a reduction reaction on the surface of the aluminum powder or aluminum alloy powder, improve sinterability and prevent a decrease in thermal conductivity, the Mg amount / oxygen amount needs to be greater than 0.1 and less than 2.0.

[0024] (Mode 4) The aluminum powder product for metal laminate molding of Mode 4 is preferably, in Modes 1 to 3, wherein the oxygen amount is 0.05 mass % or more and 0.3 mass % or less.

[0025] The range of the Mg content is specified, and the range of the oxygen content is set according to the substantial ratio, that is, the ratio of the Mg content to the oxygen content. In particular, the upper limit is specified as a value that can be obtained in consideration of the method for preparing the powder for laminated molding. The oxygen content may be 0.05 mass % or more and 0.3 mass % or less. The same may also be applied to the following modes 5 to 10.

[0026] (Mode 5) The aluminum powder product for metal laminate molding of Mode 5 is preferably, in Modes 1 to 4, a volume-based 50% cumulative particle size measured by a laser diffraction scattering method of 10 μm or more and 100 μm or less.

[0027] By setting the volume-based 50% cumulative particle size to be 10 μm or more and 100 μm or less, it is possible to provide aluminum powder having a particle size that is advantageous in aluminum powder lamination and a particle size that is preferred in the binder spraying method. The volume-based 50% cumulative particle size may be 10 μm or more and 50 μm or less. This method may also be used in the following methods 6 to 10.

[0028] (Method 6) The method for manufacturing an aluminum powder molded object of method 6 is as follows: the steps of stacking aluminum powder and applying ink containing a binder (the binder is used to selectively fix the stacked aluminum powder) are repeated alternately, and then the aluminum powder molded body is molded by heating and curing the resin in the binder, and then the aluminum powder molded body is heated and degreased to produce an aluminum powder degreased body as a sintering precursor, and the aluminum powder degreased body is heated and sintered to obtain the aluminum molded object. As the aluminum powder, an aluminum powder product for metal stacking molding is used, in which the purity of aluminum in the whole powder is 98 mass% or more, and Mg is contained in an amount of 0.01 mass% or more and 0.5 mass% or less, and the ratio of the amount of Mg (mass%) to the amount of oxygen (mass%), that is, the amount of Mg / oxygen, is set to 0.1 or more and 2.0 or less. The degreasing step is preferably carried out at a temperature below 500°C in any of an oxidizing atmosphere, an inert atmosphere, or a reduced pressure atmosphere of 1 Pa or more and 100 kPa or less.

[0029] When degreasing aluminum powder containing 0.01 mass % or more and 0.5 mass % or less of Mg and setting the value of Mg amount / oxygen amount to 0.1 or more and 2.0 or less, the oxidation of Mg can be prevented by the above-mentioned conditions of the degreasing process and the Mg can be heated and sintered. That is, the oxidation of Mg in the degreasing process is prevented, and the Mg in a state without an oxide film is maintained until the heating and sintering. Therefore, the destructive effect of the aluminum film based on Mg can be effectively exerted to obtain the effect of improving sinterability. The aluminum powder molded object can be a heat sink with fins.

[0030] (Mode 7) The method for producing an aluminum powder molded object according to Mode 7 is that, in Mode 6, an aluminum powder raw material containing 0.1 mass % or more and 1.0 mass % or less of Si in addition to the above-mentioned Mg can be used.

[0031] When an aluminum powder raw material containing Si is used, the melting point of the aluminum alloy can be lowered due to the addition of Si, which contributes to the improvement of sinterability.

[0032] (Method 8) The method for manufacturing an aluminum powder molded object involved in Method 8 is the following method: repeating the steps of stacking aluminum powder and applying ink containing an adhesive (the adhesive is used to selectively fix the stacked aluminum powder), then forming an aluminum powder molded body by heating and curing the resin, and then, preparing an aluminum powder degreased body as a sintering precursor by heating and degreasing the aluminum powder molded body, and obtaining an aluminum molded object through the step of heating and sintering the aluminum powder degreased body. As the aluminum powder, a mixture of aluminum powder with a purity of 99% or more and aluminum alloy powder containing 0.1% by mass to 1.0% by mass of Mg and 3.0% by mass to 12.0% by mass of Si is used, and the ratio of the amount of Mg (mass %) to the amount of oxygen, i.e., Mg amount / oxygen amount, is set to 0.1 to 2.0 for an aluminum powder product for metal laminate molding. The degreasing process is carried out at a temperature below 500°C in an oxidizing atmosphere, an inert atmosphere, or a reduced pressure atmosphere of 1 Pa to 100 kPa, and heating and sintering are performed while preventing oxidation of Mg.

[0033] By preventing oxidation of Mg in the degreasing process, Mg can be maintained without an oxide film until the heating and sintering. Therefore, the effect of destroying the aluminum film by Mg can be effectively exerted to obtain the effect of improving sinterability.

[0034] When the aluminum alloy powder is mixed with aluminum powder having a purity of 99% or more, in addition to 0.1% by mass to 1.0% by mass of Mg, 3.0% by mass to 12.0% by mass of Si may be contained. As long as the Si content is within the above range, it helps to lower the melting point of the aluminum alloy powder, improve sinterability, and, without significantly reducing the electrical conductivity, it is possible to manufacture an aluminum molded object that maintains high thermal conductivity.

[0035] (Method 9) The method for manufacturing an aluminum powder molded object involved in Method 9 is that, in Methods 6 to 8, the heating and sintering process can be carried out in any of an inert gas flow, a reducing gas flow, an inert gas flow under a reduced pressure atmosphere of not less than 1 Pa and not more than 100 kPa, or a reducing gas flow under a reduced pressure atmosphere of not less than 1 Pa and not more than 100 kPa.

[0036] By performing heating and sintering in any of an inert gas flow, a reducing gas flow, an inert gas flow under a reduced pressure atmosphere of 1Pa to 100kPa, or a reducing gas flow under a reduced pressure atmosphere of 1Pa to 100kPa, the added Mg can efficiently react with the aluminum oxide film to promote the formation of spinel, thereby contributing to the improvement of sinterability. In addition, when heating and sintering are performed in the above-mentioned gas flow, a sufficient amount of gas flow can be obtained, so that the binder residue can be effectively removed.

[0037] (Mode 10) The method for manufacturing an aluminum shaped object according to Mode 10 is characterized in that, in Modes 6 to 9, the oxidizing atmosphere in the degreasing step can be set to dry air having a dew point of 10° C. or less.

[0038] By using dry air with a dew point of 10°C or less, the reaction between moisture in the air and aluminum can be suppressed, and the binder component that may be contained in the aluminum powder molded body can be effectively removed. The oxidizing atmosphere in the degreasing step is preferably dry air with a dew point of -80°C or more and 0°C or less.

[0039] The relative density of the aluminum powder molded object obtained by the method for manufacturing the aluminum powder molded object can be above 90%, and the thermal conductivity can be 180 W / K.

[0040] According to the aluminum powder product for metal laminate molding involved in each aspect of the present invention, it is possible to manufacture an aluminum component having few internal defects and high relative density by a binder spraying method.

[0041] As a result, the obtained aluminum sintered body can achieve high density, high electrical conductivity, and high thermal conductivity. This can further improve the performance of heat exchange components, conductive components, and strength components manufactured using the binder spraying method, for example. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 1 is a diagram showing an example of an aluminum powder product for metal laminate molding and a sintering process thereof according to the first embodiment. Figure 1 (a) is a partially enlarged cross-sectional view showing a laminate of aluminum powder, Figure 1 (b) is an explanatory diagram showing a state where the same laminate is sintered in a heating furnace. Figure 1 (c) is an explanatory diagram showing the outline of the obtained sintered body, Figure 1 (d) is an explanatory diagram showing a state where the sintered body is subjected to final processing.

[0043] Figure 2 An example of the process of sintering aluminum powder products for metal laminate molding is shown. Figure 2 (a) is an explanatory diagram showing an aluminum powder product for metal lamination molding before sintering, Figure 2 (b) is an explanatory diagram showing the state of liquid phase wetting and expansion during the sintering process, Figure 2 (c) is an explanatory diagram showing a state where the powders are integrated into a sintered body after sintering. DETAILED DESCRIPTION

[0044] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the embodiments described below.

[0045] As an example, the aluminum powder product for metal laminate molding involved in the present embodiment is characterized in that it is an aluminum powder with a purity of 98% or more, the powder contains Mg in an amount of 0.01 mass % or more and 0.5 mass % or less, and the ratio of the amount of Mg (mass %) to the amount of oxygen (mass %), i.e., Mg amount / oxygen amount, is 0.1 or more and 2.0 or less.

[0046] Furthermore, the aluminum powder product for metal laminate molding involved in this embodiment can be a powder mixture of aluminum powder with a purity of 99% or more and aluminum alloy powder containing 0.1 mass % or more and 1.0 mass % or less of Mg and 3.0 mass % or more and 12.0 mass % or less of Si.

[0047] In the case where the aluminum powder product for metal laminate molding is a powder mixture of aluminum powder having a purity of 99% or more and aluminum alloy powder containing Mg in an amount of 0.1 mass % or more and 1.0 mass % or less, it is preferred to uniformly mix the aluminum alloy powder with the aluminum powder having a purity of 99% or more on the basis of adjusting the amount of the aluminum alloy powder so as to contain Mg in a ratio of 0.01 mass % or more and 0.5 mass % or less relative to the total mass of the powder.

[0048] The aluminum powder product for metal laminate molding contains Mg as described above, and contains Si in the above range as required, but the remainder is composed of inevitable impurities and aluminum.

[0049] [Mg: 0.01 mass% to 0.5 mass%]

[0050] By including Mg in the above range in the aluminum powder product for metal laminate molding, Mg reduces the oxide film on the surface of the aluminum powder and locally destroys the oxide film, thereby improving the sinterability of the entire aluminum powder.

[0051] Furthermore, in order to achieve the reduction reaction on the surface of the aluminum powder, a certain amount of Mg relative to the amount of oxygen is required. When the amount of Mg is too small, the oxide film of the aluminum powder cannot be partially destroyed. When the amount of Mg is too large, the sintering effect caused by the destruction of the oxide film is reduced, resulting in a decrease in electrical conductivity and thermal conductivity due to the increase in the amount of Mg.

[0052] In order to achieve a reduction reaction on the surface of the aluminum powder, improve sinterability, and prevent a decrease in thermal conductivity, it is important to set the ratio of the amount of Mg (mass %) to the amount of oxygen (mass %) contained in the aluminum powder, i.e., Mg amount / oxygen amount, to greater than 0.1 and less than 2.0.

[0053] In the method of adding Mg as an alloy component to aluminum, by adding Mg at a ratio of 0.1 to 2.0 relative to the amount of oxygen, it can react with the oxide film on the surface of the aluminum powder to form spinel (MgAl2O4), which can partially destroy it, thereby obtaining high sinterability.

[0054] When the value of Mg amount / oxygen amount is less than 0.1, there is insufficient Mg for the aluminum oxide film, and thus the oxide film destruction effect based on the spinel generation cannot be fully obtained. When the value of Mg amount / oxygen amount is greater than 2.0, there is excessive Mg for the oxide film destruction effect, which will evaporate excessively during heating and sintering under reduced pressure, thereby causing pores to form in the aluminum molded object, which may reduce the achieved density (reached density) of the aluminum molded object.

[0055] Furthermore, in the aluminum powder product for metal laminated modeling, the oxygen content is preferably 0.3 mass % or less. When the oxygen content is greater than 0.3 mass %, the oxide film may become too thick, which may make it difficult to cause local oxide film damage due to Mg addition. It is preferred that the oxygen content in the aluminum powder product for metal laminated modeling is lower, but when the oxygen content is less than 0.05 mass %, the management of manufacturing conditions becomes strict, so the oxygen content is preferably 0.05 mass % or more.

[0056] [Si: 0.1 mass% to 1.0 mass%]

[0057] In addition to the above-mentioned range of Mg, the aluminum powder product for metal lamination molding may also contain 0.1 mass % or more and 1.0 mass % or less of Si as an alloy component. As long as the Si content is within the above-mentioned range, it helps to lower the melting point of the aluminum alloy powder, improve the sinterability, and maintain high thermal conductivity without significantly reducing the electrical conductivity.

[0058] [Mg: 0.1 mass% to 1.0 mass% and Si: 3.0 mass% to 12.0 mass% of the aluminum alloy powder]

[0059] The aluminum powder for laminated molding of this embodiment may be a powder mixture of aluminum powder having a purity of 99% or more and aluminum alloy powder containing 0.1% to 1.0% by mass of Mg and 3.0% to 12.0% by mass of Si.

[0060] [50% cumulative particle size (D50) based on volume is 10 μm or more and 100 μm or less]

[0061] The aluminum powder or the pure aluminum powder and the aluminum alloy powder constituting the above-mentioned powder mixture preferably has a volume-based 50% cumulative particle size of 10 μm or more and 100 μm or less.

[0062] If the 50% cumulative particle size on a volume basis is greater than 10 μm and less than 100 μm, a powder mixture with stable fluidity and excellent sinterability can be obtained. When the powder particle size (D50) is less than 10 μm, there is a risk of dust explosion due to decreased fluidity or powder scattering. When the powder particle size (D50) exceeds 100 μm, the specific surface area of ​​the powder particles decreases, so the sinterability of the aluminum powder mixture decreases, and it may not be possible to obtain a sufficient density as a sintered body.

[0063] [Method for producing aluminum powder sintered body]

[0064] In order to use the aforementioned aluminum powder for stacking modeling to manufacture an aluminum powder sintered body, the following method can be used: first, the above-mentioned aluminum powder is used as a raw material powder (aluminum powder product for metal stacking modeling), and an adhesive containing a thermosetting resin, a thermoplastic resin or a photocurable resin is repeatedly and selectively sprayed onto the raw material powder and stacked to make it into a shape close to the target shape, and after degreasing treatment, it is heated and sintered.

[0065] For example, high-purity aluminum powder for constituting aluminum powder products for metal laminate molding can be produced by nitrogen atomization, etc. For example, aluminum alloy powder for constituting an aluminum powder mixture can be produced from an alloy melt of a target composition by nitrogen atomization.

[0066] For example, a required amount of aluminum master alloy is added to a required amount of pure aluminum corresponding to a target composition and the mixture is put into a melting furnace to prepare an aluminum alloy melt, from which the aluminum alloy powder can be prepared by an inert gas atomization method.

[0067] The obtained aluminum powder or aluminum alloy powder can be sieved or washed to remove fine powder consisting of coarse powder or smoke, and can be used as a raw material powder after sieving to a target particle size as needed.

[0068] When the aluminum powder is stacked to obtain the target shape, the raw material powder is sprayed with ink containing a selective binder and the raw material powder is repeatedly stacked, thereby obtaining a powder molded body having a shape similar to the target product shape. The raw material powder is fixed by repeated stacking to form a shape consistent with the desired three-dimensional shape. After the raw material powder is fixed by the heated binder ink coating part, unnecessary powder removal or degreasing steps are performed as needed, for example, Figure 1 The green body 1 shown in (a) is in a cubic shape. The green body 1 is subjected to the following degreasing step.

[0069] [Degreasing process]

[0070] The degreasing step is preferably performed in an oxidizing atmosphere at 500° C. or less. Furthermore, the degreasing step is more preferably performed in an oxidizing atmosphere (air, etc.) in dry air at 500° C. or less and a dew point of 10° C. or less. By performing degreasing in dry air at a dew point of 10° C. or less, the reaction between moisture in the air and aluminum can be suppressed, and the binder contained in the aluminum powder molded body can be effectively removed.

[0071] In the degreasing process, in order to effectively remove the binder contained in the ink, it is preferred to perform the degreasing in an oxidizing atmosphere containing oxygen. On the other hand, in order to maximize the oxide film destruction effect based on the above-mentioned Mg, it is preferred that Mg exists as an alloy component or a single substance in the aluminum powder degreasing body in the state of the sintering precursor. In the stage of the aluminum powder degreasing body, it is not preferred that Mg exists as an oxide. In order to suppress the oxidation of Mg, it is more preferred to perform the degreasing process at 400°C or below.

[0072] [Heating and sintering process]

[0073] If the green body 1 is obtained, the green body 1 is Figure 1 As shown in (b), the sintered product is placed in a heating furnace 2 and heated to a temperature of 560° C. to 650° C. in a reducing atmosphere or an inert gas atmosphere as a reduced pressure atmosphere for a required sintering time.

[0074] By heating to a temperature within this range, a liquid phase is generated at the interface between the raw material powders, and the liquid phase wets and expands in a manner that fills the gaps between the raw material powders, and isotropic shrinkage can be obtained to achieve high density. In this case, in order to suppress the rapid generation of the liquid phase, it is preferred to heat at a temperature increase rate of 10°C / min or less in a temperature range of 500°C or more where the liquid phase generation starts.

[0075] Furthermore, in order to make the wetting and spreading of the liquid phase between the powder particles more stable, a two-stage or more heating process may be performed for the purpose of promoting solid phase sintering by maintaining a temperature below the liquid phase generation temperature and stabilizing the gaps between the particles.

[0076] By setting the heating and sintering process in a reduced pressure atmosphere of 1 Pa or more and 100 kPa or less, the added Mg can effectively react with the oxide film on the surface of the aluminum powder, thereby promoting the spinel formation reaction. In addition, by flowing in an inert gas or a reducing gas, the binder residue remaining in the degreased body can be effectively removed.

[0077] In a reduced pressure atmosphere of less than 1 Pa, a sufficient amount of gas flow cannot be obtained to maintain a high vacuum degree, so the sintering property may be reduced due to the influence of the binder residue. At a pressure higher than 100 kPa, due to insufficient pressure reduction, the added Mg cannot be fully evaporated and the reaction with the oxide film on the aluminum surface becomes insufficient, so that the sintering property improvement effect based on the addition of Mg cannot be obtained.

[0078] Furthermore, by using an inert gas flow or a reducing gas flow, surface oxidation of aluminum during heating and sintering can be suppressed.

[0079] Figure 2 As an example of modeling an aluminum powder mixture 3, an aluminum powder mixture is depicted in which aluminum powder particles 4 having a purity of 99% or more and aluminum alloy powder particles 5 having a lower melting point than the aluminum powder particles 4 are mixed. Figure 2 The modeling shown in FIG. 1 shows an aluminum powder mixture having four aluminum powder particles 4 and one aluminum alloy powder particle 5 , but any ratio may be used as long as the number of aluminum powder particles 4 and the number of aluminum alloy powder particles 5 meet the above-mentioned mass % ratio.

[0080] Figure 2 This is an explanatory diagram for modeling a case where the aluminum powder mixture 3 is heated to a temperature of about 560° C. to 650° C.

[0081] The melting point of pure aluminum is about 660° C. Furthermore, if eutectic alloying elements such as Mg and Si are added to pure aluminum, an aluminum alloy powder having a melting point lower than about 660° C., which is the melting point of pure aluminum, can be obtained.

[0082] exist Figure 2 In (a), for the sake of simplicity of illustration, a model structure is shown in which an aluminum powder mixture 3 is constituted by mixing pure aluminum powder particles 4 and aluminum alloy powder particles 5 at a ratio of 4:1.

[0083] And, Figure 2 The aluminum powder mixture 3 may be composed of the aluminum alloy powder particles 5 by omitting all the pure aluminum powder particles 4 shown in (a).

[0084] In the Figure 2 When the aluminum powder mixture 3 shown in (a) is heated to the above temperature, the liquid phase 6 is generated from the aluminum alloy powder particles 5 with a lower melting point, such as Figure 2 As shown in (b), the liquid phase 6 wets and spreads in the gaps between the pure aluminum powder particles 4 existing around it.

[0085] The melting point of the pure aluminum powder particles 4 is about 660°C. Therefore, the entirety of the pure aluminum powder particles 4 will not be completely melted during heating in the aforementioned temperature range. However, since a portion of the interface between the pure aluminum powder particles 4 and the portion where the liquid phase 6 wets and spreads melts and fuses with each other, if the heating is continued for a predetermined time and then cooled, a product such as Figure 2 The dense sintered body 7 is almost completely melted and integrated as shown in (c). The state of the sintered body 7 generated in the heating furnace 2 is shown in FIG. Figure 1 (c) of the paper.

[0086] As needed, such as Figure 1 As shown in (d), the obtained sintered body 7 can be finished by machining with a cutting tool 8 or surface polishing, etc., to obtain a product sintered body (aluminum powder molded object) 9.

[0087] In the sintered body 7 or the product sintered body 9, the oxygen content in the aluminum powder is less than 0.3 mass%, and it contains 0.01 mass% to 0.5 mass% of Mg, and the Mg amount / oxygen amount is in the range of 0.1 to 2.0. Therefore, during sintering, the oxide film on the surface of the aluminum powder can be effectively destroyed and sintering can be performed, thereby having a dense structure in which the liquid phase effectively fills the gaps between the pure aluminum powder particles 4.

[0088] Therefore, a high-density sintered body 7 or a product sintered body 9 having a uniform shape close to the target shape can be obtained. For example, an aluminum sintered body 7 or a product sintered body 9 having a relative density of 80% or more and a thermal conductivity of 180 W / mK or more can be obtained.

[0089] As long as it is the above-mentioned sintered body 7 or the product sintered body 9, it is possible to obtain high density and high thermal conductivity.

[0090] As a result, for example, the performance of heat exchange components, conductive components, and strength components manufactured using the sintered body 7 or the product sintered body 9 can be further improved.

[0091] The aluminum sintered body 7 or the product sintered body 9 may be subjected to surface treatment such as grinding, anodizing, plating, etc. according to the purpose.

[0092] The sintered body 7 or the finished sintered body 9 is high in density and has high thermal conductivity, and therefore is desirable as a component of a heat exchanger. The sintered body 7 or the finished sintered body 9 is dense and has high thermal conductivity, and therefore using these contributes to improving the performance of the constructed heat exchanger.

[0093] Example

[0094] The required amount of aluminum master alloy corresponding to the target composition was added and put into a melting furnace to prepare aluminum alloy melt, and aluminum alloy powders of the compositions shown in Table 1 (Examples 1 to 6, Comparative Example 1, Comparative Example 2) were prepared from the melt by inert gas atomization.

[0095] Furthermore, the required amount of pure aluminum or aluminum master alloy corresponding to the target composition is prepared and put into multiple melting furnaces to produce pure aluminum melt or aluminum alloy melt, and pure aluminum powder (powder 1) and aluminum alloy powder (powder 2) of each composition shown in Table 2 are produced from the melt in each of these melting furnaces by inert gas atomization.

[0096] The obtained pure aluminum powder and aluminum alloy powder are sieved or washed to remove coarse powder or fine powder composed of smoke, etc., and then sieving corresponding to the target particle size is carried out as needed, and then pure aluminum powder (powder 1) and aluminum alloy powder (powder 2) are mixed in the mixing ratio shown in the following Table 2 to obtain an aluminum powder mixture.

[0097] Aluminum powders of the compositions listed in Tables 1 and 2 were molded into a shape of 10 mm in length × 10 mm in width × 5 mm in thickness using a metal binder jetting lamination molding device (manufactured by Digital Metal, product name: DM-P2500), and then resin cured by heating at 250° C. in an air atmosphere or an inert gas atmosphere. The degreased body was then degreased by heating at 400° C. in a dry air atmosphere with a dew point of 10° C. or less or in a humidified air atmosphere bubbled in a water tank. Furthermore, a sintered body was produced by heating at 565° C. to 650° C.

[0098] The measuring methods of each physical property value are as follows.

[0099] [Measurement of particle size distribution]

[0100] The particle size distribution of pure aluminum powder and aluminum alloy powder was measured by wet method using MT3300EXII (laser diffraction scattering particle size distribution measuring device) manufactured by MicrotracBEL Corp., and the 50% volume reference frequency cumulative diameter D50 was calculated from the obtained results.

[0101] [Modeling Density]

[0102] The bulk density of the obtained object was measured according to the JIS Z 8807 solid density and specific gravity determination method, and the true density of the object was measured by the pycnometer method. The relative density of the object (= bulk density / true density) was calculated from the obtained bulk density and true density.

[0103] [Aluminum purity, alloy element mass ratio]

[0104] The mass ratios of Mg and Si contained in aluminum powder, aluminum alloy powder, and aluminum powder mixture were measured using an inductively coupled plasma emission spectrometer. In addition, the mass ratios of 15 elements, namely, Fe, Cu, Mn, Zn, Ti, Cr, Zr, B, Ni, Bi, Pb, Ga, V, Sn, and Be, were measured simultaneously, and the value obtained by subtracting the total amount of the 17 elements including Mg and Si from 100% was defined as the aluminum purity.

[0105] [Oxygen concentration]

[0106] The oxygen concentration in the aluminum powder mixture was measured using the inert gas fusion-infrared absorption method.

[0107] [Thermal conductivity]

[0108] The thermal conductivity of the sintered body was measured by a laser flash method using LFA467 manufactured by NETZSCH Co., Ltd. The results are summarized in Tables 1 to 3 below.

[0109] [Table 1]

[0110]

[0111] [Table 2]

[0112]

[0113] [Table 3]

[0114]

[0115] As shown in Table 1, Examples 1 to 7 are samples in which aluminum contains 0.02 mass % to 0.45 mass % of Mg and 0.03 mass % to 0.25 mass % of Si, and the value of the Mg amount / oxygen amount is set to 0.1 or more and 2.0 or less.

[0116] Examples 1 to 7 have excellent relative densities ranging from 0.88 to 0.95, and show excellent thermal conductivities of 181 to 225 W / K.

[0117] Of these Examples, Comparative Example 1 containing 0.53 mass % of Mg had an excessively high Mg content and an excessively large value of Mg amount / oxygen amount, resulting in a decrease in thermal conductivity.

[0118] In Comparative Example 2, since the value of the Mg amount / oxygen amount is too small, the relative density of the sintered body becomes low and the thermal conductivity also decreases.

[0119] Examples 8 to 14 shown in Table 2 are aluminum powders for stacking molding, which are composed of a powder mixture formed by mixing aluminum powder (powder 1) having a purity of more than 99% and aluminum alloy powder (powder 2) at the powder mixing ratio shown in Table 2 (expressed as a ratio of powder 1: powder 2 or a ratio of powder 2 / powder 1).

[0120] As shown in Table 3, Examples 8 to 14 are samples in which the aluminum powder mixture contains 0.33% to 1.42% Si in addition to 0.019% to 0.15% Mg, and the value of Mg amount / oxygen amount is set to 0.13 or more and 1.10 or less.

[0121] Examples 8 to 14 had excellent relative densities ranging from 0.915 to 0.966, and showed excellent thermal conductivities of 180 W / K to 220 W / K.

[0122] Industrial Applicability

[0123] According to the aluminum powder product for metal lamination molding involved in the method of the present invention, it is possible to manufacture aluminum parts with few internal defects and high relative density by means of a binder spraying method. As a result, the obtained aluminum sintered body can obtain high density and high electrical conductivity and high thermal conductivity. Thus, the performance of heat exchange parts, conductive parts, and strength parts manufactured by, for example, the binder spraying method can be further improved. Therefore, the present invention can be used in industry.

[0124] Explanation of symbols

[0125] 1- green body, 2- heating furnace, 3- aluminum powder mixture (aluminum powder product for metal stacking molding), 4- pure aluminum powder, 5- aluminum alloy powder, 6- liquid phase, 7- sintered body, 9- product sintered body (aluminum powder molding object).

Claims

1. An aluminum powder product for metal stacking molding, characterized in that: The purity of aluminum in the entire powder is greater than 98 mass%, and it contains Mg in an amount of greater than 0.01 mass% and less than 0.5 mass%, and the ratio of the amount of Mg to the amount of oxygen, i.e., Mg amount / oxygen amount, is greater than 0.1 and less than 2.0, wherein the unit of the amount of Mg is mass % and the unit of the amount of oxygen is mass %.

2. The aluminum powder product for metal stacking molding according to claim 1, characterized in that: In addition to the above-mentioned Mg, 0.1 mass% to 1.0 mass% of Si is contained.

3. The aluminum powder product for metal stacking molding according to claim 1 or 2, characterized in that: The aluminum powder product for metal laminate molding is a mixture of aluminum powder with a purity of 99% or more and aluminum alloy powder containing 0.1% by mass or more and 1.0% by mass or less of Mg and 3.0% by mass or more and 12.0% by mass or less of Si. The ratio of the amount of Mg to the amount of oxygen contained, that is, the amount of Mg / the amount of oxygen contained is 0.1 or more and 2.0 or less, wherein the unit of the amount of Mg is mass % and the unit of the amount of oxygen is mass %.

4. The aluminum powder product for metal stacking molding according to any one of claims 1 to 3, characterized in that: The oxygen amount is 0.05 mass % or more and 0.3 mass % or less.

5. The aluminum powder product for metal stacking molding according to any one of claims 1 to 4, characterized in that: The 50% cumulative particle size on a volume basis measured by a laser diffraction scattering method is 10 μm or more and 100 μm or less.

6. A method for manufacturing an aluminum powder molded object, characterized in that: The method for manufacturing an aluminum powder molded object comprises repeating the steps of laminating aluminum powder and applying ink containing a binder, then heating and curing the resin in the binder to form an aluminum powder molded body, then heating and degreasing the aluminum powder molded body to produce an aluminum powder degreased body as a sintering precursor, and then heating and sintering the aluminum powder degreased body to obtain the aluminum molded object. The adhesive is used to selectively fix the stacked aluminum powders. As the aluminum powder, an aluminum powder product for metal laminate molding is used, wherein the purity of aluminum in the entire powder is 98% by mass or more, and the content of Mg is 0.01% by mass or more and 0.5% by mass or less, and the ratio of the amount of Mg to the amount of oxygen, i.e., the amount of Mg / oxygen, is set to 0.1 or more and 2.0 or less, wherein the unit of the amount of Mg is mass%, and the unit of the amount of oxygen is mass%. The degreasing step is performed at 500° C. or lower.

7. The method for manufacturing an aluminum powder molded object according to claim 6, wherein: Aluminum powder containing 0.1 mass % or more and 1.0 mass % or less of Si in addition to the above-mentioned Mg is used.

8. A method for manufacturing an aluminum powder molded object, characterized in that: The method for manufacturing an aluminum powder molded object comprises repeating the steps of laminating aluminum powder and applying ink containing a binder, then heating and curing a resin to form an aluminum powder molded body, then heating and degreasing the aluminum powder molded body to produce an aluminum powder degreased body as a sintering precursor, and then heating and sintering the aluminum powder degreased body to obtain an aluminum molded object. The adhesive is used to selectively fix the stacked aluminum powders. As the aluminum powder, a mixture of aluminum powder having a purity of 99% or more and an aluminum alloy powder containing 0.1% by mass or more and 1.0% by mass or less of Mg and 3.0% by mass or more and 12.0% by mass or less of Si is used, and the ratio of the amount of Mg to the amount of oxygen, i.e., the amount of Mg / oxygen, is set to 0.1 or more and 2.0 or less, and an aluminum powder product for metal laminate molding is used, wherein the unit of the amount of Mg is mass%, and the unit of the amount of oxygen is mass%. The degreasing step is performed at 500° C. or lower in any one of an oxidizing atmosphere, an inert atmosphere, and a reduced pressure atmosphere of 1 Pa to 100 kPa.

9. The method for manufacturing an aluminum powder molded object according to any one of claims 6 to 8, characterized in that: The heating and sintering step is performed in any one of an inert atmosphere, a reducing atmosphere, an inert atmosphere under a reduced pressure atmosphere of 1 Pa to 100 kPa, and a reducing atmosphere of 1 Pa to 100 kPa.

10. The method for manufacturing an aluminum powder molded object according to any one of claims 6 to 9, characterized in that: The oxidizing atmosphere in the degreasing step is dry air having a dew point of 10° C. or lower.