Thin film containing silicon and oxygen
By adding an appropriate amount of niobium to the film, the atomic ratio of niobium to silicon is controlled to form a thin film containing silicon, oxygen and niobium, which solves the problems of long reaction time and low productivity in the prior art, and improves fluorine content in a short time The adhesion of the compound film and the effect of maintaining water repellent and oil repellent properties for a long time.
Patent Information
- Application Number
- CN202280093779.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, the hydrolysis and condensation reactions of silane coupling agent treatment require dozens of hours, resulting in low productivity and additional heating and humidification treatments are required after forming a film of fluorine-containing compound, increasing process and equipment requirements.
By adding niobium to the film, the atomic ratio between niobium and silicon is controlled to be between 0% and 25%, and X-ray photoelectron spectroscopy is used to form a thin film containing silicon, oxygen and niobium, and radically assisted sputtering is used to determine the film. Or other deposition techniques to improve the adhesion of the film.
In a short period of time, the adhesion of fluorine-containing compound films is significantly improved, and the water repellent, oil repellent or sliding properties are maintained for a long time, reducing the subsequent processing process and equipment requirements.
Smart Images

Figure CN118984886A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thin film containing at least silicon and oxygen. Background Art
[0002] In order to improve the water repellency, oil repellency or sliding property of the surface of a substrate such as glass or plastic, a thin film of a fluorine-containing compound is formed on the surface of the substrate. The hydroxyl groups OH on the surface of the substrate are combined with the silane coupling agent contained in the fluorine-containing compound through a condensation reaction, thereby improving the adhesion (see Non-Patent Document 1).
[0003] Prior art literature
[0004] Non-patent literature
[0005] Non-patent document 1: Journal of the Japanese Adhesion Society, Vol. 52, No. 1, 2016, pp. 9-15, “Control of hydrolysis and condensation reaction in silane coupling agent treatment”, Yoshinobu Nakamura, Nozomu Karu, Masayo Noda, Hideji Fujii Summary of the invention
[0006] Problems to be solved by the invention
[0007] However, in order to obtain sufficient adhesion through the hydrolysis and condensation reaction of the above-mentioned silane coupling agent treatment, a reaction time of up to tens of hours is required, so there is a problem in productivity. In addition, after forming the film of the fluorine-containing compound, if post-treatment such as heating and humidification is performed, the reaction can be promoted, but it is necessary to add a step for post-treatment such as heating and humidification, or to set dedicated equipment.
[0008] An object of the present invention is to provide a thin film containing silicon and oxygen, which can improve the adhesion of a thin film containing a fluorine compound in a short time.
[0009] Means for solving problems
[0010] The present invention solves the above-mentioned problems by a thin film containing silicon and oxygen, wherein the thin film contains silicon, oxygen and niobium, and the atomic number ratio (Nb / Si) of the above-mentioned niobium to the above-mentioned silicon is 0% to 25% (excluding the two end points) obtained by atomic number measurement using X-ray photoelectron spectroscopy.
[0011] Effects of the Invention
[0012] According to the present invention, the adhesion of a thin film of a fluorine-containing compound can be improved in a short time. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a cross-sectional view showing one embodiment of the substrate covering film of the present invention.
[0014] Figure 2This is a cross-sectional view showing another embodiment of the substrate covering film of the present invention.
[0015] Figure 3 This is a cross-sectional view showing an example of a sputtering device used in the thin film production method of the present invention. DETAILED DESCRIPTION
[0016] The present invention includes: a thin film of the first invention, which contains silicon, oxygen and niobium as elements; a substrate coating film of the second invention, which includes the thin film of the first invention and a thin film composed of a fluorine-containing compound; a substrate coating film of the third invention, which further includes an optical film in the substrate coating film of the second invention; and a manufacturing method of the fourth invention, which manufactures the thin film of the first invention.
[0017] The film of the first invention contains silicon, oxygen and niobium, and the atomic ratio (Nb / Si) of the niobium to silicon obtained by atomic number measurement using X-ray photoelectron spectroscopy is 0% to 25% (excluding both end points). That is, 0% < atomic ratio (Nb / Si) < 25%. As shown in the results of the examples and comparative examples described later, if the atomic ratio Nb / Si of niobium to silicon is 0%, that is, niobium is not contained, the adhesion of the film composed of the fluorine-containing compound becomes low. In addition, if the atomic ratio Nb / Si of niobium to silicon is 25% or more, the adhesion of the film composed of the fluorine-containing compound becomes low. On the other hand, if the atomic ratio Nb / Si of niobium to silicon is 0% to 25% (excluding both end points), the adhesion of the film composed of the fluorine-containing compound becomes high, and the performance of the fluorine-containing compound film such as water repellency, oil repellency or sliding property can be maintained for a long time.
[0018] The thin film containing silicon and oxygen of the first invention can be formed on the main surface of the thin film composed of a fluorine-containing compound. In addition, the thin film containing silicon and oxygen of the first invention can be formed between the thin film composed of a fluorine-containing compound and the substrate. Thus, the following substrate coating film, i.e., the substrate coating film of the second invention, can be formed: the substrate coating film includes the thin film containing silicon and oxygen of the first invention formed on the surface of the substrate, and a thin film composed of a fluorine-containing compound formed on the surface of the thin film containing silicon and oxygen of the first invention. The second invention is formed by Figure 1 The illustrated embodiment will be described.
[0019] In addition, the thin film containing silicon and oxygen of the first invention can be formed between the thin film composed of a fluorine-containing compound and the optical film. Thus, the following substrate coating film, i.e., the substrate coating film of the third invention, can be formed: the substrate coating film includes an optical film formed on the surface of the substrate, the thin film containing silicon and oxygen of the first invention formed on the surface of the optical film, and a thin film composed of a fluorine-containing compound formed on the surface of the thin film containing silicon and oxygen of the first invention. The third invention is formed by Figure 2The illustrated embodiment will be described.
[0020] The thin film containing silicon and oxygen in the first invention is not particularly limited, and the film thickness can be 0.1 nm to 5 nm.
[0021] The thin film containing silicon and oxygen of the first invention can be produced by the fourth invention, wherein the first target is silicon or silicon oxide (oxidized niobium), the second target is niobium or niobium oxide (oxidized niobium), oxygen is used as a radical source, and a film is formed by a radical-assisted sputtering method. Figure 3 The illustrated embodiment will be described.
[0022] Hereinafter, one embodiment of the present invention described above will be described based on the drawings. Figure 1 1 is a cross-sectional view showing an embodiment of the substrate coating film of the present invention, wherein a substrate coating film 2 is formed on the surface of a substrate 1. The substrate 1 may be an organic glass substrate or other plastic substrates, an inorganic glass substrate or other inorganic substrates, a stainless steel substrate or other metal substrates, etc., without particular limitation, and substrates of various materials may be used.
[0023] The substrate coating film 2 of this example is composed of: a thin film 21 containing silicon and oxygen formed on the surface of the substrate 1; and a thin film 22 composed of a fluorine-containing compound formed on the surface of the thin film 21 containing silicon and oxygen. The thin film 21 containing silicon and oxygen is the thin film of the first invention described above, and contains silicon, oxygen and niobium, and the atomic number ratio of niobium to silicon (Nb / Si) obtained by atomic number measurement using X-ray photoelectron spectroscopy is 0% to 25% (excluding both end values).
[0024] The thin film 21 containing silicon and oxygen can be used Figure 3 The sputtering device 3 shown in the figure uses silicon or silicon oxide as the first target, niobium or niobium oxide as the second target, and oxygen as the radical source to form a film by radical-assisted sputtering. Figure 3 The sputtering apparatus shown in FIG. 1 is briefly described, but the thin film containing silicon and oxygen of the first invention is not limited to the one using Figure 3 The sputtering device 3 shown in the figure forms the film by a sputtering method, but the film may be formed by other methods such as CVD (Chemical Vapor Deposition), ALD (Atomic Layer Deposition), PLD (Palsed Laser Deposition), vacuum evaporation, etc.
[0025] Figure 31 is a cross-sectional view showing an example of a sputtering device for the method for manufacturing a thin film of the present invention. The sputtering device 3 of this example is a device capable of implementing a radical assisted sputtering (RAS) method, and is provided with a vacuum chamber 31 which is a hollow body in a substantially rectangular parallelepiped shape. An exhaust pipe and a vacuum pump (not shown) are connected to the vacuum chamber 31, and the interior of the vacuum chamber 31 can be maintained at a predetermined vacuum degree. In addition, a cylindrical substrate holder 32 is rotatably provided inside the vacuum chamber 31, and a substrate 1 to be film-formed is held on its outer peripheral surface.
[0026] Two sputtering sources 33 and 34 and one plasma source 35 are arranged around a substrate holder 32 disposed inside a vacuum chamber 31. Each sputtering source 33 and 34 has an electrode such as a magnetron sputtering electrode, and a target is mounted on the surface of each electrode when film formation is performed. An AC power source 331 and 341 are connected to each electrode via a transformer that adjusts the power, and an AC voltage of, for example, about 1k to 100kHz is applied. The plasma source 35 of this example includes: a housing 351 fixed in a manner that blocks an opening formed on the wall surface of the vacuum chamber 31; and a dielectric module 352 including an antenna fixed to the housing 351. The dielectric module 352 including the antenna is connected to a high-frequency power source 353. In addition, the antenna receives power supply from the high-frequency power source 353 to generate an induced electric field inside the vacuum chamber 31, thereby generating plasma.
[0027] A film forming process area 332 is formed in front of the sputtering source 33, and a film forming process area 342 is formed in front of the sputtering source 34. The film forming process area 332 on one side is surrounded by partition walls 333 protruding from the inner wall of the vacuum chamber 31 toward the substrate holder 32, so that independent spaces can be ensured inside the vacuum chamber 31. The film forming process area 342 on the other side is also surrounded by partition walls 343 protruding from the inner wall of the vacuum chamber 31 toward the substrate holder 32, so that independent spaces can be ensured inside the vacuum chamber 31.
[0028] Similarly, a reaction process area 354 is formed in front of the plasma source 35. The reaction process area 354 is also surrounded in all directions, vertically, horizontally, and horizontally, by a partition wall 355 protruding from the inner wall of the vacuum chamber 31 toward the substrate holder 32, similarly to the film forming process areas 332 and 342, and a space independent of the film forming process areas 332 and 342 is ensured inside the vacuum chamber 31. In the sputtering device 3 of this example, the processes in the film forming process areas 332 and 342 and the reaction process area 354 are configured to be independently controllable.
[0029] It should be noted that each sputtering source 33, 34 is connected to a sputtering gas supply system, and the flow rate of the supplied sputtering gas is adjusted by a mass flow controller and introduced into each film forming process area 332, 342 through piping. In addition, a reaction treatment gas supply system 356 is connected to the plasma source 35, and the flow rate of the supplied reaction treatment gas is adjusted by a mass flow controller and introduced into the reaction process area 354 through piping. Figure 3 In the figure, reference numeral 36 is provided adjacent to the vacuum chamber 31 and is a load lock chamber for switching the atmosphere pressure, and is used for carrying in and out substrates before and after processing.
[0030] In order to form a sputtering device 3 with such a configuration Figure 1 The thin film 21 containing silicon and oxygen is formed on the surface of the substrate 1 as shown in the figure. First, silicon or silicon oxide is installed as a first target on the electrode of one sputtering source 33, and niobium or niobium oxide is installed as a second target on the electrode of the other sputtering source 34. Then, the interior of the vacuum chamber 31 is set to, for example, 10 -1 ~10 -5 The substrate holder 32 holding the substrate 1 is rotated at a constant speed while the inert gas as the sputtering gas is supplied to the two film forming process areas 332 and 342, and the oxygen gas as the reaction gas is supplied to the reaction process area 354. In addition, the two sputtering sources 33 and 34 are supplied with power from an AC power supply, and the plasma source 35 is supplied with power from a high frequency power supply.
[0031] Thus, by the sputtering treatment in the two continuous film forming process areas 332 and 342, an intermediate thin film containing silicon and niobium is formed on the surface of the substrate 1, and by the plasma exposure treatment in the subsequent reaction process area 354, the intermediate thin film undergoes film conversion and becomes an ultra-thin film. Then, by repeatedly performing two sputtering treatments and plasma exposure treatments, an ultra-thin film is deposited on the ultra-thin film, and such treatment is repeated until the final thin film 2 is formed. It should be noted that the thin film 21 containing silicon and oxygen in this example is not particularly limited, and can be set to a film thickness of about 0.1nm to 5nm.
[0032] return Figure 1 The substrate coating film 2 of this example has a thin film 22 composed of a fluorine-containing compound formed on the surface of a thin film 21 containing silicon and oxygen. The thin film 2 composed of the fluorine-containing compound has the function of improving the water repellency, oil repellency or sliding property of the surface of the substrate 1, inhibiting the adhesion of pollutants such as hand fat, and facilitating the removal of attached pollutants. The thin film 2 composed of the fluorine-containing compound of this example can be set to an appropriate film thickness according to the purpose, for example, it can be set to a film thickness of about 0.1nm to 20nm.
[0033] The fluorine-containing compound of this example is not particularly limited, and examples thereof include organic compounds containing fluorine groups such as alkoxysilane compounds having a perfluoropolyether group. Examples of the alkoxysilane compound having a perfluoropolyether group include: 1 -R 2 -(CH2) m -Si(OR 3 )3 represented by the compound.
[0034] Here, R 1 It represents a linear or branched fluoroalkyl group (having, for example, 1 to 20 carbon atoms) in which one or more hydrogen atoms in the alkyl group are replaced by fluorine atoms, and preferably represents a perfluoroalkyl group in which all hydrogen atoms in the alkyl group are replaced by fluorine atoms. 2 The structure of the repeating structure including at least one perfluoropolyether (PFPE) group is preferably a structure of the repeating structure including two PFPE groups. Examples of the repeating structure of the PFPE group include a repeating structure of a linear PFPE group and a repeating structure of a branched PFPE group. Examples of the repeating structure of the linear PFPE group include -(OC n F 2n ) p - (n represents an integer of 1 to 20, and p represents an integer of 1 to 50. The same shall apply hereinafter). Examples of the repeating structure of the branched PFPE group include -(OC(CF3)2) p -Structure represented by, and -(OCF2CF(CF3)CF2) p As the repeating structure of the PFPE group, preferably a repeating structure of a straight chain PFPE group is mentioned, and more preferably -(OCF2) p -and-(OC2F4) p -. R 3 represents an alkyl group having 1 to 4 carbon atoms, and preferably represents a methyl group. m represents an integer greater than 1. In addition, m is preferably an integer less than 20, more preferably less than 10, and further preferably less than 5.
[0035] Among such alkoxysilane compounds having a perfluoropolyether group, it is preferred to use CF3-(OCF2) q -(OC2F4) r -O-(CH2)3-Si(OCH3)3. Here, q represents an integer from 1 to 50, and r represents an integer from 1 to 50. As the alkoxysilane compound having a perfluoropolyether group, a commercially available product can be used. Examples of such commercially available products include OPTOOL UD509 (the above-mentioned CF3-(OCF2) q -(OC2F4) r-O-(CH2)3-Si(OCH3)3, manufactured by Daikin Industries, Ltd.). In addition, the alkoxysilane compound having a perfluoropolyether group can be used alone or in combination of two or more. It should be noted that the method for forming the thin film 22 composed of the fluorine-containing compound in this example is not particularly limited, and can be formed by a spray method, a vacuum evaporation method, a CVD method, etc., and is more preferably formed by a vacuum evaporation method.
[0036] In this way, by forming a thin film 21 containing silicon and oxygen on the surface of the substrate 1, and then forming a thin film 22 composed of a fluorine-containing compound on the surface of the thin film 21, the adhesion of the thin film 22 composed of the fluorine-containing compound to the substrate 1 becomes higher, and as a result, the water repellency, oil repellency or sliding property exerted by the thin film 22 composed of the fluorine-containing compound can be maintained for a long time.
[0037] Figure 2 2 is a cross-sectional view showing another embodiment of the substrate covering film of the present invention, wherein a substrate covering film 2 is formed on the surface of a substrate 1. Figure 1 Similarly to the embodiment shown, organic glass substrates and other plastic substrates, inorganic glass substrates and other inorganic substrates, stainless steel and other metal substrates, etc. can be used without particular limitation, and substrates of various materials can be used.
[0038] The substrate covering film 2 of this example is composed of: an optical film 23 formed on the surface of the substrate 1, a thin film 21 containing silicon and oxygen formed on the surface of the optical film 23, and a thin film 22 composed of a fluorine-containing compound formed on the surface of the thin film 21 containing silicon and oxygen. Figure 1 The substrate covering film 2 of the embodiment shown is different in that an optical film 23 is formed between the substrate 1 and the thin film 21. The thin film 21 containing silicon and oxygen and the thin film 22 composed of a fluorine-containing compound are similar in structure to the above-mentioned thin film 21. Figure 1 The embodiments shown are identical, so reference is made here to their description.
[0039] The optical film 23 in this example refers to a film that reflects, transmits, or absorbs a specific wavelength range by utilizing interference and absorption of the film. It is not particularly limited, and in addition to optical filters such as bandpass filters and anti-reflection films, there are also decorative films that adjust the color tone of visible light. For example, the optical film 23 as an anti-reflection film can be manufactured by stacking a plurality of thin films composed of silicon oxide and a thin film composed of niobium oxide or silicon nitride.
[0040] In this way, an optical film 23 is formed on the surface of the substrate 1, a thin film 21 containing silicon and oxygen is formed on the surface of the optical film 23, and a thin film 22 composed of a fluorine-containing compound is further formed on the surface of the thin film 21. The thin film 22 composed of a fluorine-containing compound has higher adhesion to the optical film 23. As a result, the water repellency, oil repellency or sliding property of the thin film 22 composed of a fluorine-containing compound can be maintained for a long time.
[0041] Example
[0042] Hereinafter, the present invention will be described by giving examples that further embody the present invention. However, the numerical values and specific examples of the configuration shown below do not limit the present invention.
[0043] 《Example 1》
[0044] An antireflection film (optical film 23 ) having the film composition shown in Table 1 was formed on the surface of a glass substrate 1 (gorira 3, Corning Incorporated) under the film forming conditions shown in Table 2 using a sputtering device (RAS-2200, manufactured by SHINCRON, with a vapor deposition function).
[0045] [Table 1]
[0046] Substrate / Membrane Film thickness(nm) Glass substrate 1 - <![CDATA[Silicon dioxide (SiO2)]]> 10 <![CDATA[Silicon nitride (Si3N4)]]> 18.15 <![CDATA[Silicon dioxide (SiO2)]]> 28.45 <![CDATA[Silicon nitride (Si3N4)]]> 129.81 <![CDATA[Silicon dioxide (SiO2)]]> 15.51 <![CDATA[Silicon nitride (Si3N4)]]> 34.33 <![CDATA[Silicon dioxide (SiO2)]]> 22.06 <![CDATA[Silicon nitride (Si3N4)]]> 134.89 <![CDATA[Silicon dioxide (SiO2)]]> 83.58
[0047] [Table 2]
[0048]
[0049] Next, a thin film 21 containing silicon and oxygen was formed on the surface of the antireflection film (optical film 23) with a film thickness of 0.25 nm using a sputtering device (RAS-2200 manufactured by SHINCRON, with a vapor deposition function) under the conditions shown in Table 3. Next, a resistor boat containing a fluorine-containing compound (OPTOOL UD509 manufactured by Daikin Corporation) was heated on the surface of the antireflection film (optical film 23) using a sputtering device (RAS-2200 manufactured by SHINCRON, with a vapor deposition function) to form a thin film 22 composed of a fluorine-containing compound with a film thickness of about 7 nm by vapor deposition.
[0050] Within 1 hour after film formation, the substrate coating film 2 formed on the glass substrate 1 was subjected to a friction test to measure the contact angle as an evaluation item of adhesion. In the friction test, a friction tester (Three ream abrasion tester manufactured by SHINCRON) was used to apply a load of 1000 kg to steel wool (BONSTAR#0000 of Japan Steel Wool Company) to a 1 cm square of the film surface with a stroke of 40 mm at a speed of 60 round trips per minute for 2000 times. The contact angle was measured using a contact angle meter (DM-500 manufactured by Kyowa Interface Science Co., Ltd.) to measure the contact angle of the friction surface.
[0051] In parallel with the friction test, the number of atoms of silicon, niobium, and oxygen contained in the thin film 21 containing silicon and oxygen was measured. First, an X-ray photoelectron spectrometer (PHI5000 Versa Probe III manufactured by ULVAC-PHI) was used to perform an argon gas etching treatment for several seconds on the substrate coating film 2 formed on the glass substrate 1 until the atomic number % of fluorine was less than 10%, thereby substantially removing the thin film 22 formed on the thin film 21. When the atomic number % of fluorine was less than 10%, the atomic numbers of silicon, niobium, and oxygen were measured. Table 3 shows the atomic numbers of silicon, niobium, and oxygen contained in the thin film 21 when two sputtering sources (equivalent to 10) were used to form the thin film 21. Figure 3 The graphs show the power (kW) supplied to the electrodes (33, 34) of the sputtering device 3, the flow rate of argon gas for sputtering, the flow rate of oxygen gas for reaction, and the film formation time. The graphs also show the contact angle after friction, the atomic ratio of niobium to silicon (Nb / Si), and the atomic ratio of oxygen to the sum of the atomic numbers of niobium and silicon (O / (Nb+Si)).
[0052] 《Example 2 to Example 5》
[0053] As shown in Table 3, the power (kW) supplied to the electrodes of the two sputtering sources, the flow rate of the reaction oxygen gas, and the film formation time were appropriately changed to change the atomic ratio of niobium to silicon (Nb / Si) in Examples 2 to 5, and the contact angle after friction was measured in the same manner as in Example 1.
[0054] 《Comparative Example 1, Comparative Example 2》
[0055] As shown in Table 3, by appropriately changing the power (kW) supplied to the electrodes of the two sputtering sources, the flow rate of the reaction oxygen gas, and the film formation time, Comparative Example 1 in which the atomic ratio of niobium to silicon (Nb / Si) was set to 0% and Comparative Example 2 in which the atomic ratio of niobium to silicon (Nb / Si) was set to 25.0% were prepared, and the contact angle after friction was measured in the same manner as in Example 1.
[0056] [Table 3]
[0057]
[0058] "think"
[0059] As shown in the results of Table 3 above, when the atomic ratio of niobium to silicon (Nb / Si) is 0% and 25%, as in Comparative Examples 1 and 2, the contact angle after the friction test is less than 100°. A small contact angle means that the water repellency, oil repellency or sliding property originally possessed by the thin film 22 composed of the fluorine-containing compound is reduced, which means that the thin film 22 is peeled off during the friction test. Therefore, when the atomic ratio of niobium to silicon (Nb / Si) is 0% and 25%, the thin film 22 composed of the fluorine-containing compound has low adhesion to the anti-reflection film (optical film 23). In contrast, when the atomic ratio of niobium to silicon (Nb / Si) is 0% to 25% (excluding the two end values of 0% and 25%), as in Examples 1 to 5, the contact angle after the friction test is greater than 100°, so it is confirmed that the thin film 22 composed of the fluorine-containing compound has high adhesion to the anti-reflection film (optical film 23).
[0060] It should be noted that, in the above-mentioned embodiments and examples, an example of adding niobium to a thin film containing silicon and oxygen is cited, but instead of the above-mentioned niobium, any one element of vanadium (V), tantalum (Ta), titanium (Ti), zirconium (Zr), hafnium (Hf), aluminum (Al), gallium (Ga), indium (In), tungsten (W), molybdenum (Mo), chromium (Cr), zinc (Zn), yttrium (Y), scandium (Sc), tin (Sn), bismuth (Bi), and nickel (Ni) (these are referred to as Group M) or two or more elements in Group M. The range of the value of the preferred atomic number ratio M / Si in this case can be easily determined by conducting experiments with reference to the above-mentioned embodiments and comparative examples.
[0061] Explanation of symbols
[0062] 1...Substrate
[0063] 2…Substrate coating film
[0064] 21…Thin film containing silicon and oxygen
[0065] 22…Thin films composed of fluorinated compounds
[0066] 23…Optical film
[0067] 3…Sputtering device
[0068] 31…Vacuum chamber
[0069] 32…Substrate holder
[0070] 33、34···Sputtering source
[0071] 331, 341…AC power supply
[0072] 332, 342…Film forming process area
[0073] 333, 343…partition wall
[0074] 35…Plasma source
[0075] 351···Housing
[0076] 352…Dielectric module
[0077] 353…High frequency power supply
[0078] 354…Reaction process area
[0079] 355…partition wall
[0080] 356…Reaction treatment gas supply system
Claims
1. A thin film containing silicon and oxygen, comprising silicon, oxygen and niobium, wherein the atomic number ratio of niobium to silicon, i.e., Nb / Si, obtained by atomic number measurement using X-ray photoelectron spectroscopy is 0% to 25%, and the ratio does not include any end points. 2 . The thin film containing silicon and oxygen according to claim 1 , which is formed on a main surface of a thin film composed of a fluorine-containing compound. 3 . The thin film containing silicon and oxygen according to claim 1 , which is formed between a thin film composed of a fluorine-containing compound and a substrate. 4 . The thin film containing silicon and oxygen according to claim 1 , which is formed between a thin film composed of a fluorine-containing compound and an optical film. 5 . The thin film containing silicon and oxygen according to claim 1 , wherein the film thickness is 0.1 nm to 5 nm.
6. A substrate coating film, comprising: The thin film containing silicon and oxygen according to any one of claims 1 to 5 formed on a surface of a substrate; and A thin film composed of a fluorine-containing compound is formed on the surface of the thin film containing silicon and oxygen.
7. A substrate coating film, comprising: An optical film formed on a surface of a substrate; The thin film containing silicon and oxygen according to any one of claims 1 to 5 formed on the surface of the optical film; and A thin film composed of a fluorine-containing compound is formed on the surface of the thin film containing silicon and oxygen.
8. A method for producing a thin film, wherein: The thin film containing silicon and oxygen according to any one of claims 1 to 5 is produced by a radical-assisted sputtering method using silicon or silicon oxide as the first target, niobium or niobium oxide as the second target, and oxygen as a radical source.