Pollution-resistant internal pressure type hollow fiber membrane material and preparation method thereof
By regulating the viscosity and flow rate ratio of the inner surface of the hollow fiber membrane, the smoothness of the membrane surface is achieved, and the problem that existing membrane materials are prone to form polluted layers in polluted environments is solved, the film's pollution resistance and cleaning efficiency are improved, and the film is extended. The service life of the membrane.
Patent Information
- Application Number
- CN202410773550.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-11-22
AI Technical Summary
When existing membrane materials are used in contaminated environments, it is easy to form contaminated layers that are difficult to clean, resulting in increased filtration resistance, reduced flux and shortened life. It is difficult for existing modification technologies to achieve uniform hydrophilic distribution and pollution resistance on the membrane surface. sex.
By regulating the viscosity ratio and extrusion speed ratio of polymer solution and core solution, matching the flow rate of polymer solution and core solution, a smooth hollow fiber membrane on the inner surface is prepared, reducing the adsorption and deposition of pollutants and improving the film's pollution resistance sex.
It effectively improves the pollution resistance and cleaning efficiency of the membrane material, extends the stability and life of the membrane, and reduces the cost of water treatment.
Smart Images

Figure CN118987998A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane materials, and in particular to a pollution-resistant internal pressure hollow fiber ultrafiltration and microfiltration membrane material and a preparation method thereof. Background Art
[0002] Porous organic membrane materials have become mainstream in the fields of tap water purification, industrial wastewater and municipal sewage. The water quality of various water sources varies greatly, but the common point is that they contain suspended particulate matter, dissolved organic matter, etc. The presence of these pollutants is an important challenge to the use of membrane materials. In recent years, domestic membrane materials have developed on a large scale, and the cost of materials has dropped significantly. However, when applied to large-scale water treatment processes such as municipal water treatment, the market requires membrane materials to be resistant to pollution and stable in operation, so as to have low water treatment costs. Pollution-resistant membrane materials are characterized by a high recovery rate of membrane performance after cleaning, and stable or slow attenuation of membrane flux during operation.
[0003] When using membranes to purify tap water or sewage, bacteria, viruses, suspended matter, and particulate impurities need to be filtered out to obtain a clear, sterile, and virus-free water source. The interception of these pollutants means that the pollutants will be concentrated in the water and may be deposited on the membrane surface to form a filter cake layer, which greatly increases the filtration resistance, increases energy consumption, and increases the probability of forming a difficult-to-clean membrane contamination layer. The contamination of membrane materials leads to a decrease in membrane permeability, requiring more frequent chemical cleaning, and the life of the membrane material is also reduced. To solve the stability and durability of these membrane materials during use, the generally adopted solutions include: First, add a pretreatment process to the front end of the ultrafiltration membrane, such as flocculation sedimentation, ozone sterilization, and security filters to reduce the degree of contamination of the rear-end ultrafiltration membrane. This type of solution increases the complexity and cost of the process, and a small amount of pollutants still enter the membrane section after treatment. The second type of solution is to improve the pollution resistance of the membrane material to prevent pollutants from being adsorbed and accumulated on the membrane surface.
[0004] There are a lot of patent reports on how to improve the pollution resistance of membrane materials. For example, hydrophilic polymer materials, such as cellulose acetate polymers, are used. However, the disadvantage of such polymers is that they have poor resistance to acids, alkalis and oxidants. After the membrane is polluted, strong acids, strong alkalis and strong oxidizing chemicals are often used to clean the membrane, and the life of the membrane material is relatively short. Therefore, the most successful solution is to use hydrophobic polymers and hydrophilic materials to hybridize or blend to achieve hydrophilicity of the material.
[0005] Patent CN1579601 discloses that a hydrophilic hollow fiber membrane is obtained by blending a polyvinylidene fluoride hollow fiber membrane with a hydrophilic macromolecule such as polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone and / or polyethylene oxide. Patent CN1579602 discloses a hydrophilic method for blending sintered α-alumina / polyvinylidene fluoride with an asymmetric structure. Patent CN1687222 discloses the hydrophilic modification of polyvinylidene fluoride blended with titanium dioxide. Adding inorganic materials to the membrane solution improves the hydrophilicity of polyvinylidene fluoride, but since polyvinylidene fluoride and these inorganic materials cannot form crosslinks at a microscopic angle, the hydrophilicity of the membrane material cannot be ensured. Patent CN101269302 discloses a method for hydrophilizing membrane materials through polyvinyl pyrrolidone polymers. However, since polyvinyl pyrrolidone polymers are water-soluble polymers, most of them are lost during the film-forming process. The hydrophobicity of the polyvinylidene fluoride polymer used is very strong, so the final membrane material has limited improvement in pollution resistance. Patent 2010101309368 discloses the use of hydrophilic polymers and hydrophobic polymers such as polyether sulfone, polyvinyl chloride, polyaryl sulfide, polycarbonate, polyacrylonitrile, polyimide, polyetherimide or polyamide hybridization to achieve the purpose of permanent hydrophilicity. The hydrophobicity of the polymer selected in the patent is weaker than that of polyvinylidene fluoride polymer, but the pollution resistance is still limited. The key problem of this type of hydrophilic modification scheme is that the hydrophilic area on the membrane surface is difficult to be evenly distributed at a mesoscopic or microscopic angle, so pollutants can always find the hydrophobic area on the membrane surface, and adsorb and deposit on the membrane surface under the action of non-chemical bonds, forming pollution accumulation.
[0006] Patent CN1594405 discloses a method for hydrophilic modification of membrane materials by chemical grafting copolymerization. This technology adopts grafting acrylic acid on the membrane surface, and then adopts a diacrylate type crosslinking agent to obtain a surface hydrophilic membrane material. Patent CN1704152 discloses a method for preparing a hydrophilic microporous membrane by dip coating modification. The prepared microporous membrane has good hydrophilicity and high water flux, and can reduce the adsorption of biologically active substances such as proteins. Patent CN1772359 provides a chemical modification technology for grafting groups with hydrophilic properties and ion exchange properties on the surface of hollow fiber microfiltration membranes and flat microfiltration membranes. These modification technology processes are relatively complicated, and the covalent bonds formed are not resistant to acid, alkali and oxidation cleaning in industrial processes. The performance stability of the membrane material in long-term operation cannot be guaranteed. In addition, the degree of surface modification, such as the degree of grafting (the amount of grafted groups per square micrometer), is difficult to accurately control, so the performance of the membrane surface cannot be accurately regulated. For example, there may be local areas where hydrophilic groups are not grafted, and then the pollutants will interact with the hydrophobic polymer material and cause membrane contamination. Surface modification methods also include the use of zwitterionic coating or grafting methods (Acta Biomaterialia, 2016, 40 (142-152), but similar to the disclosed patent technology, the surface pollution resistance is not durable and cannot withstand chemical cleaning. Whether it is coated or chemically grafted to the membrane surface, these hydrophilic groups have the above-mentioned shortcomings. These chemical bonds have a limited lifespan under the action of chemical cleaning and oxidizing agents. With the loss of hydrophilic groups, the pollution resistance of the membrane material decreases.
[0007] Therefore, it is very important to achieve membrane pollution resistance from a physical rather than chemical perspective. One of the physical means is to design a smooth, uniform and low-roughness membrane surface. According to the principle of fluid mechanics transfer, the water flow velocity on the surface of a general object is zero. This is the basic assumption of chemical transfer and fluid mechanics. The direct result is that there is a water flow boundary layer on the surface. In this boundary layer, the flow rate from the membrane surface to the main solution gradually increases from zero to the main water flow velocity. During the membrane filtration process, pollutants can easily stay and accumulate in this water flow boundary layer, resulting in membrane pollution. If the membrane surface is rough, the surface uniformity is poor, the boundary layer thickness increases, and the membrane pollution is aggravated. Therefore, improving the pollution resistance of membrane materials from the perspective of membrane surface morphology design is a neglected but very important direction in the field.
[0008] The hollow fiber membrane has two surfaces, the inner surface and the outer surface. If an external pressure hollow fiber membrane material is prepared, the morphology of the outer surface needs to be adjusted, otherwise the inner surface needs to be designed. During the hollow fiber spinning process, the polymer solution is extruded from the spinneret, passes through an air section and enters the external gel bath. Through the exchange of solvent and water, phase separation is achieved to obtain a solidified membrane material. During the extrusion process, there is also a core liquid inside the hollow fiber, which is the inner gel bath; the core liquid and the polymer solution are extruded at the same time, and the exchange of water and solvent is achieved from the inside to achieve phase separation. The phase separation of the hollow fiber membrane is carried out from both the inside and the outside, which determines that we can adjust the structure of the inner and outer surfaces of the hollow fiber membrane separately according to needs.
[0009] It is relatively easy to achieve smoothness and low roughness on the outer surface, which is related to the preparation process of the hollow fiber membrane. The polymer solution has a viscosity several orders of magnitude higher than that of water. When the polymer solution is extruded into the water, the water is under normal pressure. The polymer solution is equivalent to a solid in a very short contact time, and the water will not cause a large disturbance to the polymer solution. Since there is no impact between water and the polymer solution, the outer surface of the hollow fiber is relatively smooth. We can adjust the outer pore structure and surface smoothness of the membrane by adjusting the height of the spinneret from the water surface, the composition of the solvent in the external gel bath, the temperature, etc.
[0010] However, it is very difficult to achieve a smooth inner surface. During the extrusion of the polymer solution from the spinneret, the high viscosity solution is extruded from a millimeter-level slit, which will cause high shear pressure; when it comes out of the spinneret, the core liquid is also extruded at the same time, and there may be a large difference in the flow rates of the two. The core liquid is generally mainly water or a mixture of water and solvent, and its volume is small. During the phase separation process, its solvent content increases, thereby slowing down the phase separation rate. At this time, the polymer solution has not yet solidified, and the surface of the solution may be impacted by the core liquid to form wavy ripples, so that the membrane surface appears rough. How to avoid this phenomenon has always been a key issue that has plagued membrane preparation. Summary of the invention
[0011] The present invention goes beyond the perspective of material chemistry and starts from the perspective of material physics. It achieves the purpose of pollution resistance by changing the physical morphology of the membrane surface, that is, the smoothness or roughness of the membrane surface, thereby avoiding the preferential adsorption and deposition of suspended particles and dissolved organic matter on the membrane surface. This method does not change the chemical properties of the main membrane material, so it has strong tolerance to chemical cleaning, and is a simple and effective new means to improve the pollution resistance of membrane materials. The above invention has been neglected in the field of membrane preparation for a long time, and its regulation method is also difficult. Therefore, the present invention proposes to achieve the improvement of the smoothness of the inner surface of the membrane and the reduction of membrane pollution by regulating the match between the viscosity / flow rate of the polymer solution (i.e., the membrane making liquid) and the viscosity and flow rate of the core liquid, which is an important innovation in the field.
[0012] The first object of the present invention is to provide a method for preparing a pollution-resistant internal pressure hollow fiber ultrafiltration membrane, the preparation method comprising the following steps:
[0013] (1) preparing a polymer solution as a membrane-forming solution and a core liquid, wherein the viscosity ratio of the core liquid to the membrane-forming solution is 1:1-300;
[0014] (2) extruding the membrane-forming liquid prepared in step (1) through the outer cavity of the coaxial spinneret; and at the same time, extruding the core liquid prepared in step (1) through the inner cavity of the coaxial spinneret; during the extrusion process, the ratio of the membrane-forming liquid extrusion speed to the core liquid extrusion speed is 1-2:1, thereby obtaining an initial hollow fiber membrane;
[0015] (3) placing the initial hollow fiber membrane obtained in step (2) into a gel bath for solidification;
[0016] (4) The solidified hollow fiber membrane is rinsed to remove the solvent and additives, and then dried to obtain the hollow fiber membrane.
[0017] Furthermore, the core liquid in step (1) is an aqueous solution of polyvinyl alcohol, polyethylene glycol, xanthan gum, guar gum, polyvinyl pyrrolidone, polyacrylic acid, polymaleic acid, polydiallyl quaternary ammonium salt, or polyacrylamide; and the viscosity of the core liquid is adjusted to be greater than 1 centipoise.
[0018] Furthermore, the viscosity can be adjusted by adding a viscosity modifier such as polyethylene glycol, glycerol, ethylene glycol, propylene glycol, etc. to the core liquid.
[0019] Furthermore, the core liquid in step (1) also includes a solvent for the membrane-making liquid. This operation can better adjust the pore size of the inner surface of the hollow fiber membrane when necessary, and add an appropriate amount of solvent to the core liquid, including one of nitrogen-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, trimethyl phosphate or triethyl phosphate; the amount of solvent added depends on the design of the pore size of the membrane, and generally the larger the pore size, the higher the amount of solvent added, and the mass percentage of the solvent added to the membrane-making liquid in the core liquid is 0 to 80%, preferably 0 to 60%.
[0020] Furthermore, the polymer material in the membrane-forming solution of step (1) is a hydrophobic polymer. Preferably, the hydrophobic polymer is selected from one or more combinations of polysulfone, polyethersulfone, polyvinyl chloride, polyaryl sulfide, polyacrylonitrile, polyimide, polyetherimide, and semi-crystalline polymer polyvinylidene fluoride.
[0021] Furthermore, the solvent of the membrane-forming solution in step (1) is selected from one or a mixture of nitrogen-methylpyrrolidone, dipyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, trimethyl phosphate or triethyl phosphate.
[0022] Furthermore, the membrane-forming solution in step (1) further comprises a pore-forming agent, and the pore-forming agent is selected from a small molecule pore-forming agent and / or a macromolecular pore-forming agent;
[0023] The small molecule pore-forming agent is selected from one or more combinations of ethanol, propanol, butanol, ethylene glycol, diethylene glycol, polyethylene glycol, glycerol, lithium chloride, magnesium chloride, and calcium chloride;
[0024] The weight ratio of the small molecule pore-forming agent to the polymer material is 0.05-2.0:1, preferably, the weight ratio of the small molecule pore-forming agent to the polymer material is 0.1-0.8:1;
[0025] The macromolecular pore-forming agent is selected from one or more combinations of polyethylene glycol, polyvinyl alcohol, and polyvinyl pyrrolidone, and the average molecular weight of the macromolecular pore-forming agent is 1-3 million Daltons, preferably, the average molecular weight is 2-2 million Daltons;
[0026] The weight ratio of the macromolecular pore-forming agent to the polymer material is 0.01-2:1. Preferably, the weight ratio of the macromolecular pore-forming agent to the polymer material is 0.05-0.5:1.
[0027] Furthermore, before the initial hollow fiber membrane enters the gel bath in step (3), it also includes passing through an air section, the temperature of the air section is 10-90°C, preferably, the temperature of the air section is 20-60°C; the relative humidity of the air section is 40-100%, preferably, the relative humidity of the air section is 50-95%.
[0028] Furthermore, the medium of the gel bath in step (3) is water or a mixture of water and a solvent of the film-making liquid; when the medium of the gel bath is a mixture of water and a solvent of the film-making liquid, the content of the solvent of the film-making liquid is not higher than 80%; the temperature of the gel bath is 10-95°C, preferably, the temperature of the gel bath is 20-90°C.
[0029] The second object of the present invention is to provide a pollution-resistant internal pressure hollow fiber ultrafiltration membrane, wherein the pollution-resistant internal pressure hollow fiber ultrafiltration membrane is prepared by the aforementioned preparation method.
[0030] Furthermore, the inner surface roughness of the pollution-resistant internal pressure hollow fiber ultrafiltration membrane is in the range of 10-100 nanometers.
[0031] The pore size of the pollution-resistant internal pressure hollow fiber ultrafiltration membrane of the present invention is in the range of ultrafiltration and microfiltration, and the molecular weight cutoff of the membrane is in the range of 10,000 Daltons to 2,000,000 Daltons.
[0032] For the internal pressure hollow fiber membrane, the feature of the present invention is to control the viscosity of the core liquid and the speed of the core liquid extrusion to match the viscosity and extrusion speed of the polymer solution, so as to achieve the purpose of controlling the morphology of the inner surface of the hollow fiber membrane. The core liquid composition of the hollow fiber membrane is generally a mixed solution of water and solvent. According to the thermodynamics of phase separation, adding a certain amount of solvent to the core liquid can inhibit the diffusion of the solvent into the water. Before the polymer solution separates to form a polymer-rich phase and a polymer-poor phase, the concentration of the polymer will decrease, thereby increasing the opening filtration and pore size of the membrane surface. Adding solvent will dilute the polymer concentration and significantly reduce the polymer concentration at the interface of the core liquid and the polymer solution. These conditions are likely to affect the morphology of the inner surface of the hollow fiber spinning.
[0033] For the polymer solution system prepared by ultrafiltration and microfiltration hollow fiber membrane, in many cases, there are problems such as low smoothness of membrane surface and insufficient pollution resistance of membrane material. The above-mentioned defects in the principle of hollow fiber membrane preparation and the demand for membrane performance in the application of hollow fiber membrane materials for large-scale components are the starting point of the present invention.
[0034] In many cases, technicians do not take the above factors into consideration and base the performance test of hollow fiber membranes on a few simple parameters such as pore size, water permeability, hydrophilicity, and strength, ignoring the importance of the morphology of the inner surface of the hollow fiber to the pollution resistance of the membrane material during use.
[0035] There is a very simple principle in the membrane transfer process: when the liquid flows over the membrane surface, a velocity boundary layer is formed. In the velocity boundary layer, the interface velocity close to the membrane is zero, while the velocity close to the interface of the liquid body is consistent with the main body velocity. The liquid velocity in the velocity boundary layer changes with the velocity gradient. This phenomenon is closely related to the morphology of the membrane surface. If the membrane surface is rough, the velocity boundary layer on the membrane surface will be amplified. During the membrane filtration process, suspended particles and dissolved organic matter accumulate on the membrane surface driven by the water flow, especially when the membrane surface is rough, forming a pollution layer with greater resistance. When the membrane is backwashed, the cleaning effect of the area with greater resistance is worse, that is, the backwash flux of the polluted area is lower, which leads to the actual cleaning effect of the polluted area being worse than expected, which will lead to continuous accumulation of pollution, thereby reducing the filtration stability of the membrane. According to this principle, the ideal membrane filtration surface should be uniform and smooth to avoid uneven accumulation of pollutants under the action of the velocity boundary layer.
[0036] In order to form a smooth membrane surface, the present invention reduces the flow rate and viscosity difference between the polymer solution and the core liquid. The first step is to increase the viscosity of the core liquid. When the viscosity of the core liquid is greatly different from the viscosity of the polymer solution, we can adjust the flow rate of the polymer solution and the core liquid by the design of the nozzle and the flow rate of the pump, thereby reducing the interface impact generated when the two solutions are in contact and causing the roughness of the membrane surface to increase. Therefore, we prefer that the ratio of the viscosity of the polymer solution to the viscosity of the core liquid is in the range of 10-300. The second point is to reduce the contact between the core liquid and the polymer solution to avoid the reduction of the polymer concentration at the interface, or to increase the viscosity of the polymer at the interface to avoid the formation of a rough surface. The ratio of the extrusion speed of the polymer solution and the core liquid is preferably 1-2:1.
[0037] The strategy proposed by the present invention is to use a core liquid component with a viscosity greater than 1 centipoise (viscosity of water), preferably with a viscosity between 10-1000 centipoise. The core liquid is a single component or a mixture of multiple components; including polyvinyl alcohol, polyethylene glycol, xanthan gum, guar gum, polyvinyl pyrrolidone, polyacrylic acid, polymaleic acid, polydiallyl quaternary ammonium salt, polyacrylamide, polyethylene glycol, glycerol, ethylene glycol, propylene glycol, etc. The amount of addition used is determined according to the viscosity ratio a value of the polymer solution and the core liquid, and the general value is 1-300:1. The above selection is not an exhaustive list. For those skilled in the art, the above concept can be extended to any liquid that meets the above conditions.
[0038] Beneficial effects of the present invention:
[0039] The present invention controls the morphology of the inner surface of the hollow fiber membrane by screening the components of the membrane-making liquid and the core liquid, and screening the viscosity ratio and extrusion speed ratio of the membrane-making liquid and the core liquid, thereby obtaining hollow fiber ultrafiltration and microfiltration membrane materials with smooth inner surfaces. The pollution resistance of the membrane material can be effectively improved, the cleaning efficiency and the stability of the membrane can be enhanced, and the cost of use can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 .An electron microscope photograph of the inner surface of the polysulfone ultrafiltration membrane.
[0041] Figure 2 .This is an electron microscope photograph of the inner surface of the polysulfone ultrafiltration membrane.
[0042] Figure 3 . Polysulfone ultrafiltration membrane prepared in Example 1 and Comparative Example 1
[0043] A is an electron microscope photo of the inner surface of a smooth polyethersulfone ultrafiltration membrane after gray water test;
[0044] B is an electron microscope photograph of the inner surface of a rough-surfaced polyethersulfone ultrafiltration membrane after gray water test;
[0045] C is the change of membrane mass transfer resistance over time during the filtration of synthetic gray water by a smooth-surface polyethersulfone ultrafiltration membrane;
[0046] D is the variation of membrane mass transfer resistance of polyethersulfone membrane with high rough inner surface during filtration of synthetic grey water. DETAILED DESCRIPTION
[0047] The present invention is further explained below with reference to the examples, but the examples do not limit the present invention in any form.
[0048] Example 1
[0049] Prepare polymer solution: 200 g of polyethersulfone (polymer material) and 10 g of polyethylene glycol (molecular weight 20,000 Daltons, macromolecular pore-forming agent) are dissolved in a mixed solvent of 750 g of dimethylacetamide (solvent) and 60 g of diethylene glycol (small molecule pore-forming agent) at 90°C with sufficient stirring.
[0050] After the polymer is completely dissolved, it is filtered through a stainless steel wire mesh with a pore size of 40 microns, and is placed in an oven at 50°C for degassing to obtain a polymer solution with a viscosity of 4600 centipoise.
[0051] Preparation of core liquid: The core liquid is a mixed solution of 150 g of dimethylacetamide (solvent for membrane-making liquid), 10 g of guar gum, 100 g of glycerol (viscosity regulator) and 650 g of water. The viscosity of the core liquid is measured to be 27 centipoise, and the viscosity ratio of the polymer solution to the core liquid is 170.
[0052] The polymer solution is extruded together with the core liquid in the central tube of the spinneret through a jacketed spinneret. The extrusion speed of the polymer solution and the core liquid is 0.25m / s. It passes through an air section controlled at a temperature of 25°C and a humidity of 55% for about 0.4 seconds, enters a water bath at a temperature of 30oC, enters the water washing area after gel solidification, and then is wound and collected.
[0053] The measured membrane outer diameter is 1.35 mm, the inner diameter is 0.82 mm, and the pure water flux is 650 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.03 microns, the root mean square roughness is 8.7 nm, and the inner surface of the membrane is smooth according to the scanning electron microscope structure observation. Figure 1 .
[0054] The membrane obtained in the example was subjected to a pollution filtration test. The test process was as follows: the membrane obtained in the example was used to filter a 100 ppm humic acid solution for 30 minutes and the water flux during the filtration process was tested. After the filtration was completed, the membrane was backwashed with pure water for 5 minutes to complete a cycle. After repeating 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 590 L·m -2 ·hr -1bar -1 , the water flux recovery rate is 91%, and the pollution resistance effect is excellent.
[0055] The membrane obtained in the embodiment was subjected to a synthetic ash water treatment test (the main components of the synthetic ash water are: 580ppm NaCl, 200ppm NaHCO3, 20ppm humic acid, 20ppm CaCl2, 100ppm cellulose, 100ppm kaolin, 20ppm SDS, 10ppm NH4Cl, 400ppm casein). The test process is: add 60ppm Fe2(SO4)3 to the ash water to flocculate the pre-treated ash water, mix at a speed of 100r / min for 2min, let it stand for 30min after the flocculation is completed, treat the flocculated supernatant with the membrane obtained in the embodiment for 30 minutes and test the water flux during the filtration process, and calculate the change of the mass transfer resistance of the membrane over time. It is found that the resistance of the membrane changes very little. After the pollution filtration, there is no pollutant attached to the membrane surface. Figure 3 A and C.
[0056] The above results indicate that controlling the viscosity ratio of the polymer solution to the core liquid and the extrusion flow rate ratio can effectively adjust the roughness of the inner surface of the hollow fiber membrane and obtain a contamination-resistant hollow fiber membrane.
[0057] Comparative Example 1
[0058] The polymer solution was prepared according to the formula of Example 1, and the core liquid component was changed to a mixed solution of 280 g of dimethylacetamide (solvent for membrane-making solution), 20 g of glycerol (viscosity modifier), 2 g of polyvinyl pyrrolidone, and 720 g of water. The core liquid viscosity was measured to be 2.4 centipoise, and the polymer solution to core liquid viscosity ratio was 1916. According to the method of Example 1, the extrusion speed of the polymer solution was 0.15 m / s, the extrusion speed of the core liquid was 0.35 m / s, and the hollow fiber membrane was obtained by spinning.
[0059] The measured membrane outer diameter is 1.30 mm, the inner diameter is 0.78 mm, and the pure water flux is 620 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.03 microns, the root mean square roughness is 110.2nm, and the scanning electron microscope structure observation shows that the inner surface of the membrane is not smooth and has a corrugated structure. Figure 2 .
[0060] The membrane obtained in the example was subjected to a pollution filtration test. The test process was based on Example 1. After 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 406 L·m -2 ·hr -1 bar -1 , the water flux recovery rate is 66%, and the pollution resistance effect is poor.
[0061] The membrane obtained in this comparative example was subjected to a synthetic grey water treatment test (Implementation Case 1), and the results are shown in Figure 3 B and D. The mass transfer resistance of the membrane slowly and continuously increased. After the experiment, it was found that there was a layer of contaminants on the membrane surface, with a large amount of bacteria and other particles accumulated. This shows that increasing the viscosity ratio of the polymer solution to the core liquid and the extrusion speed ratio is not conducive to forming a smooth inner surface of the hollow fiber, and the membrane material is not resistant to contamination.
[0062] Comparative Example 2
[0063] The polymer solution was prepared according to the formula of Example 1, and the core liquid component was changed to a mixed solution of 250 g of polyethylene glycol (PEG-400) and 750 g of water. The core liquid viscosity was measured to be 12 centipoise, and the polymer solution to core liquid viscosity ratio was 383. According to the method of Example 1, the polymer solution extrusion speed was 0.25 m / s, and the core liquid extrusion speed was 0.35 m / s to obtain a hollow fiber membrane. The outer diameter of the membrane was measured to be 1.44 mm, the inner diameter was 0.79 mm, and the pure water flux was 460 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.02 microns, the root mean square roughness is 125.8 nm, and scanning electron microscopy structural observation shows that the inner surface of the membrane is not smooth and the cross-sectional pore connectivity is reduced.
[0064] The membrane obtained in the example was subjected to a pollution filtration test. The test process was referred to Example 1. After 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 350 L·m -2 ·hr -1 bar -1 The water flux recovery rate is 76%, and the anti-fouling effect is worse than that of the low-roughness surface. This shows that the viscosity ratio of the polymer solution to the core liquid is high, which is not conducive to the formation of a smooth surface structure and is not conducive to slowing down membrane fouling.
[0065] Example 2
[0066] Preparation of polymer solution: 200 g of polysulfone (polymer material) and 10 g of polyvinyl pyrrolidone (molecular weight 150,000 Daltons, macromolecular pore-forming agent) were dissolved in a mixed solvent of 750 g of dimethylacetamide (solvent) and 50 g of diethylene glycol (small molecule pore-forming agent) at 75°C with sufficient stirring.
[0067] After the polymer was completely dissolved, it was filtered through a stainless steel wire mesh with a pore size of 40 microns, and allowed to stand at room temperature for degassing to obtain a polymer solution. The viscosity of the polymer solution was measured at 25°C to be 3900 centipoise.
[0068] Preparation of core liquid: The core liquid is a mixed solution of 200 grams of dimethylacetamide (solvent for membrane-making liquid), 2 grams of polyacrylic acid, 50 grams of polyvinyl alcohol and 550 grams of water. The viscosity of the core liquid is measured at 25°C to be 35 centipoise, and the viscosity ratio of the polymer solution to the core liquid is 111.
[0069] It is extruded through a jacketed spinneret together with the core liquid in the central tube of the spinneret. The extrusion speed of the polymer solution and the core liquid is 0.2m / s. It passes through an air section controlled at a temperature of 35°C and a humidity of 68% for about 0.3 seconds, enters a water bath at a temperature of 45°C, enters the water washing area after gel solidification, and then is wound and collected.
[0070] The measured membrane outer diameter is 1.28 mm, the inner diameter is 0.75 mm, and the pure water flux is 660 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.05 microns, the root mean square roughness is 10.5 nm, and scanning electron microscopy structural observation shows that the inner surface of the membrane is smooth.
[0071] The membrane obtained in the example was subjected to the synthetic grey water treatment test as in Example 1. After repeating 5 cycles, the pure water flux of the membrane was tested, and the pure water flux of the membrane was 580 L·m -2 ·hr -1 bar -1 The water flux recovery rate is 88%. The surface membrane material has good pollution resistance in a severely polluted water environment. The case shows that by using different polymer systems and pore-forming agent systems, by adjusting the viscosity and flow rate of the polymer solution and the viscosity and flow rate of the core liquid, an inner surface with low surface roughness can be obtained, which has a good pollution resistance effect.
[0072] Comparative Example 3
[0073] The polymer solution and the core liquid were prepared according to the formula of Example 2. The spinning core liquid speed in Example 2 was changed to 0.10 m / s, the extrusion speed of the polymer solution was changed to 0.55 m / s, and the other process parameters were the same as in Example 2 to obtain a hollow fiber membrane.
[0074] The measured membrane outer diameter is 1.36 mm, the inner diameter is 0.68 mm, and the pure water flux is 550 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.05 microns, the root mean square roughness is 130nm, and scanning electron microscopy structural observation shows that the inner surface of the membrane is uneven, with some areas being smooth and some areas being highly rough.
[0075] The membrane obtained in the example was subjected to a pollution filtration test. The test process was referred to Example 1. After 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 304 L·m-2 ·hr -1 bar -1 The water flux recovery rate was 55%, the flow rate difference between the core liquid and the polymer solution was too large, the membrane surface formed was rough, and the membrane was not resistant to pollution.
[0076] This comparative example shows that when the ratio of the membrane liquid extrusion speed to the core liquid extrusion speed exceeds the 1-2:1 specified in the present invention, the membrane surface roughness, uniformity and pollution resistance cannot achieve the effects of the present invention.
[0077] Example 3
[0078] Preparation of polymer solution: 160 g of polysulfone (polymer material) was dissolved in 840 g of dimethylacetamide (solvent) at 35° C. with sufficient stirring.
[0079] After the polymer was completely dissolved, it was filtered through a stainless steel wire mesh with a pore size of 40 microns, and was placed in an oven at 30°C for degassing to obtain a polymer solution. The viscosity of the polymer solution was measured to be 1704.5 centipoise.
[0080] Preparation of core liquid: The core liquid is a mixed solution of 150 g of dimethylacetamide (solvent for membrane-making liquid), 2 g of xanthan gum solution and 850 g of water. The viscosity of the core liquid measured at 25°C is 21 centipoise, and the viscosity ratio of the polymer solution to the core liquid is 81.
[0081] The polymer solution is extruded together with the core liquid in the central tube of the spinneret through a jacketed spinneret at a speed of 0.1 m / s. It passes through an air section controlled at a temperature of 26°C and a humidity of 55% for about 1 second, enters a water bath at a temperature of 30°C, enters the water washing area after gel solidification, and is then wound and collected.
[0082] The measured membrane outer diameter is 1.37 mm, the inner diameter is 0.79 mm, and the pure water flux is 280 L·m -2 ·hr -1 bar -1 The pore size in the membrane structure transitions from 0.08 to 4 μm, the root mean square roughness is 18.0 nm, and scanning electron microscopy observation shows that the membrane inner surface has low porosity but a smooth surface.
[0083] The membrane obtained in the example was subjected to a pollution filtration test. The membrane obtained in the example was used to filter a 500 ppm bovine serum protein solution for 30 minutes and the water flux during the filtration process was tested. After the filtration was completed, the membrane was backwashed with pure water for 5 minutes to complete a cycle. After repeating 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 230 L·m -2 ·hr -1 bar -1 The water flux recovery rate was 82%, and the membrane had good resistance to fouling.
[0084] Comparative Example 4
[0085] The polymer solution and the core liquid were prepared according to the formula of Example 3. The core liquid was changed to a mixture of water and solvent (65 / 35%), and the viscosity of the core liquid was measured to be about 1 centipoise.
[0086] The polymer solution is extruded together with the core liquid in the central tube of the spinneret through a jacketed spinneret. The extrusion speed of the polymer solution and the core liquid is 0.1m / s. After passing through the temperature and humidity controlled air section for about 1 second, it enters a water bath at a temperature of 30°C, enters the water washing area after gel solidification, and then is wound and collected.
[0087] The measured membrane outer diameter is 1.30 mm, the inner diameter is 0.75 mm, and the pure water flux is 293 L·m -2 ·hr -1 bar -1 The pore size in the membrane structure transitions from 0.05 to 5 μm, the root mean square roughness is 55.8 nm, and scanning electron microscopy observation shows that the connectivity between membrane pores is poor and the inner surface is uneven.
[0088] The membrane obtained in the example was subjected to a pollution filtration test, and the test process was referred to Example 3. After repeating 5 cycles, the pure water flux of the membrane was tested, and the pure water flux of the membrane was 160 L·m -2 ·hr -1 bar -1 The water flux recovery rate was 54%, and the membrane had poor resistance to fouling.
[0089] Example 4
[0090] Preparation of polymer solution: 200 g of polyetherimide (polymer material) was dissolved in a mixed solvent of 650 g of nitrogen methyl pyrrolidone (solvent) and 250 g of polyethylene glycol (PEG-400, small molecule pore-forming agent) at 120° C. with sufficient stirring.
[0091] After the polymer was completely dissolved, it was filtered through a stainless steel wire mesh with a pore size of 40 microns and then allowed to stand for degassing to be used as a polymer solution. The viscosity of the polymer solution was measured to be 9380 centipoise.
[0092] Preparation of core liquid: The core liquid is a mixed solution of 120 grams of nitrogen methyl pyrrolidone (solvent for membrane-making solution), 2 grams of polydiallyl quaternary ammonium salt, 5 grams of guar gum and 880 grams of water. The viscosity of the core liquid is measured to be 160 centipoise, and the viscosity ratio of the polymer solution to the core liquid is 58.
[0093] The polymer solution is extruded together with the core liquid in the central tube of the spinneret with a jacket. The extrusion speed of the polymer solution and the core liquid is 0.2 m / s. It passes through an air section controlled at a temperature of 15°C and a humidity of 48% for about 0.5 seconds, enters a water bath at a temperature of 10°C, enters the water washing area after gel solidification, and then is wound and collected.
[0094] The outer diameter of the membrane was measured to be 1.39 mm, the inner diameter was 0.84 mm, the pore size of the membrane was 0.03 μm, and the pure water flux was 420 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.06 microns, the root mean square roughness is 12.5 nm, and scanning electron microscopy observation shows that the inner surface of the membrane is relatively smooth.
[0095] The membrane obtained in the example was subjected to a pollution filtration test. The test process was based on Example 1. After 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 366 L·m -2 ·hr -1 bar -1 The water flux recovery rate was 87%, and the membrane had good resistance to fouling.
[0096] Comparative Example 5
[0097] Preparation of polymer solution: 100 g of polyvinylidene fluoride (polymer material), 30 g of polyvinyl pyrrolidone powder (K30, macromolecular pore-forming agent), dissolved in a mixed solvent of 720 g of N-methylpyrrolidone (solvent for membrane-forming solution) and 20 g of lithium chloride (small molecule pore-forming agent) at 80°C with sufficient stirring. The polymer solution is a uniformly mixed viscous liquid, which is placed in a 60°C oven for degassing as a polymer solution. The viscosity of the polymer solution is 7540 centipoise at 25°C.
[0098] Preparation of core liquid: The core liquid is a mixed solution of 170 g N-methylpyrrolidone, 150 g polyvinylpyrrolidone (K30) and 680 g water. The viscosity of the core liquid is measured to be 42 centipoise. The viscosity ratio of the core liquid to the viscosity of the membrane-making liquid is 1:179.
[0099] The polymer solution is extruded from the spinneret with a jacket and the core liquid in the center tube of the spinneret. The polymer solution extrusion speed is 0.4m / s, and the core liquid extrusion speed is 0.15m / s. It passes through the air section with temperature and humidity control for about 0.2 seconds, enters the water bath at a temperature of 60°C, enters the water washing area after gel solidification, and then is wound and collected. The outer diameter of the membrane is measured to be 1.52mm, the inner diameter is 0.92mm, the pore size of the membrane is a sponge-like pore of 0.04 microns, and the pure water flux is 390L·m -2 ·hr -1 bar -1The pore size of the membrane is 0.06 microns, the root mean square roughness is 61.4 nm, and scanning electron microscopy observation shows that the inner surface of the membrane has a certain degree of roughness.
[0100] The membrane obtained in the example was used to treat grey water. The test process was based on the example 4. After five cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 210 L·m -2 ·hr -1 bar -1 The water flux recovery rate was 53%, and the membrane had poor resistance to fouling.
[0101] Comparative Example 6
[0102] 150 g of polyvinyl chloride was dissolved in a mixed solvent of 750 g of nitrogen methyl acetamide, 30 g of polyvinyl pyrrolidone (K90), 40 g of polyethylene glycol (PEG-2000), and 30 g of lithium chloride (additive) at 80° C. with sufficient stirring.
[0103] The polymer solution is a uniformly mixed viscous liquid, which is placed in an oven at 60°C for degassing to obtain a polymer solution. The viscosity of the polymer solution is measured at 25°C to be 8460 centipoise.
[0104] The core liquid composition refers to Comparative Example 5 (the measured core liquid viscosity is 42 centipoise), and the viscosity ratio of the polymer solution to the core liquid is 2:1.
[0105] The polymer solution is extruded from the spinneret with a jacket together with the core liquid in the central tube of the spinneret. The polymer solution extrusion speed is 0.3m / s, the core liquid extrusion speed is 0.12m / s, and the ratio of the membrane liquid extrusion speed to the core liquid extrusion speed is 2.5:1. After about 6 seconds of air section controlled by temperature and humidity, it enters a water bath at a temperature of 25°C, enters the water washing area after gel solidification, and then is wound and collected.
[0106] The outer diameter of the membrane was measured to be 1.48 mm, the inner diameter was 0.87 mm, the pore size of the membrane was a sponge-like pore of 0.04 μm, and the pure water flux was 446 L·m -2 ·hr -1 bar -1 The pore size of the membrane is 0.04 microns, the root mean square roughness is 180 nm, and scanning electron microscopy observation shows that the inner surface of the membrane is uneven.
[0107] The membrane obtained in the example was used to treat grey water. The test process was based on the example 1. After 5 cycles, the pure water flux of the membrane was tested. The pure water flux of the membrane was 138 L·m -2 ·hr -1 bar -1The water flux recovery rate is 31%, indicating that the viscosity ratio is within 300, but the extrusion speed ratio exceeds 2:1, and the membrane has poor pollution resistance. Due to the large difference in viscosity between the polymer solution and the core liquid and the large difference in flow rate between the two, the combined effect leads to the formation of a highly rough inner surface, and it is difficult to restore the original performance of the membrane by cleaning the pollutants.
[0108] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a pollution-resistant internal pressure hollow fiber ultrafiltration membrane, characterized in that: The preparation method comprises the following steps: (1) preparing a polymer solution as a membrane-forming solution and a core liquid, wherein the viscosity of the core liquid and the viscosity of the membrane-forming solution are in a ratio of 1: 1-300; (2) extruding the membrane-forming liquid prepared in step (1) through the outer cavity of the coaxial spinneret; and at the same time, extruding the core liquid prepared in step (1) through the inner cavity of the coaxial spinneret; during the extrusion process, the ratio of the membrane-forming liquid extrusion speed to the core liquid extrusion speed is 1-2:1, thereby obtaining an initial hollow fiber membrane; (3) placing the initial hollow fiber membrane obtained in step (2) into a gel bath for solidification; (4) The solidified hollow fiber membrane is rinsed to remove the solvent and additives, and then dried to obtain the hollow fiber membrane.
2. The preparation method according to claim 1, characterized in that: The core liquid in step (1) is an aqueous solution of polyvinyl alcohol, polyethylene glycol, xanthan gum, guar gum, polyvinyl pyrrolidone, polyacrylic acid, polymaleic acid, polydiallyl quaternary ammonium salt, and polyacrylamide; the viscosity of the core liquid is adjusted to be greater than 1 centipoise.
3. The preparation method according to claim 1, characterized in that: The core liquid in step (1) also includes a solvent and / or a viscosity regulator for adding a membrane-making liquid.
4. The preparation method according to claim 3, characterized in that: The mass percentage of the solvent added to the membrane-making liquid in the core liquid is not higher than 80%.
5. The preparation method according to claim 1, characterized in that: The polymer material in the membrane-forming solution of step (1) is a hydrophobic polymer. Preferably, the hydrophobic polymer is selected from one or more combinations of polysulfone, polyethersulfone, polyvinyl chloride, polyaryl sulfide, polyacrylonitrile, polyimide, polyetherimide, and polyvinylidene fluoride.
6. The preparation method according to claim 1, characterized in that: The solvent of the membrane-forming solution in step (1) is selected from one or a mixture of nitrogen-methylpyrrolidone, dipyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, trimethyl phosphate or triethyl phosphate.
7. The preparation method according to claim 1, characterized in that: The membrane-forming solution in step (1) further comprises a pore-forming agent, and the pore-forming agent is selected from a small molecule pore-forming agent and / or a macromolecular pore-forming agent; The small molecule pore-forming agent is selected from one or more combinations of ethanol, propanol, butanol, ethylene glycol, diethylene glycol, polyethylene glycol, glycerol, lithium chloride, magnesium chloride, and calcium chloride; The weight ratio of the small molecule pore-forming agent to the polymer material is 0.05-2.0:1, preferably, the weight ratio of the small molecule pore-forming agent to the polymer material is 0.1-0.8:1; The macromolecular pore-forming agent is selected from one or more combinations of polyethylene glycol, polyvinyl alcohol, and polyvinyl pyrrolidone. The average molecular weight of the macromolecular pore-forming agent is between 1 and 3 million Daltons, and preferably, the average molecular weight is between 2 and 2 million Daltons. The weight ratio of the macromolecular pore-forming agent to the polymer material is 0.01-2:1, and preferably, the weight ratio of the macromolecular pore-forming agent to the polymer material is 0.05-0.5:
1.
8. The preparation method according to claim 1, characterized in that: Before the initial hollow fiber membrane enters the gel bath in step (3), it also includes passing through an air section, the temperature of the air section is 10-90°C, preferably, the temperature of the air section is 20-60°C; the relative humidity of the air section is 40-100%, preferably, the relative humidity of the air section is 50-95%.
9. The preparation method according to claim 1, characterized in that: The medium of the gel bath in step (3) is water or a mixture of water and a solvent of the film-making liquid; when the medium of the gel bath is a mixture of water and a solvent of the film-making liquid, the solvent content of the film-making liquid is not higher than 80%; the temperature of the gel bath is 10-95°C, preferably, the temperature of the gel bath is 20-90°C.
10. A pollution-resistant internal pressure hollow fiber ultrafiltration membrane, characterized in that: The pollution-resistant internal pressure hollow fiber ultrafiltration membrane is prepared by the preparation method described in any one of claims 1 to 9.
11. The pollution-resistant internal pressure hollow fiber ultrafiltration membrane according to claim 10, characterized in that: The inner surface roughness of the pollution-resistant internal pressure hollow fiber ultrafiltration membrane is in the range of 10-100 nanometers.
Citation Information
Patent Citations
Polyvinylidene fluoride hollow fiber membrane for hemodialysis
CN1579601A
Sintered alpha-alumina / polyviny lidene fluoride blended hollow fiber membrane preparing method and its product
CN1579602A
Method for making PH value-sensitive polyvinylidene fluoride hollow fibre intelligent film and products thereby
CN1594405A
Modification film of polyvinylidene fluoride and preparation method thereof
CN1687222A
Preparation of hydrophilic polyvinylidene fluoride microporous membrane
CN1704152A