COF / GO / ANF composite nano-channel membrane and super-assembly preparation method thereof
By combining COF, GO, and ANF membranes, a COF/GO/ANF composite nanochannel membrane with a regular and ordered structure and adjustable thickness was prepared, which solved the problems of insufficient crystallinity and mechanical strength of covalent organic framework membranes and achieved efficient ion transport.
Patent Information
- Application Number
- CN202410274767.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-22
AI Technical Summary
The crystallinity and mechanical strength of existing covalent organic framework membranes are insufficient, and the preparation of independent and easy-to-manipulate covalent organic framework membranes remains challenging, limiting their practical application in nanofluid membrane materials.
By combining covalent organic framework (COF) membranes with graphene oxide (GO) and aramid fiber (ANF) membranes, COF/GO/ANF composite nanochannel membranes were prepared via interfacial polymerization and vacuum filtration, forming a self-supporting composite membrane with a regular and ordered structure and adjustable thickness.
This improves the mechanical stability and surface charge density of the membrane, reduces the internal resistance of ion transport, and provides a promising application prospect for intelligent ion transport.
Smart Images

Figure CN118988000A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nano ion channels, and specifically relates to a COF / GO / ANF composite nano channel membrane and a super assembly preparation method thereof. Background Art
[0002] Artificial nanochannels have been widely studied in the preparation of nanofluidic devices. Bionic nanochannels have attracted great attention in the fields of nanochannel-based energy conversion, ion screening and sensing detection due to their excellent mechanical and chemical stability, adjustable structure and easily customized surface properties.
[0003] Covalent organic framework membranes have broad application prospects in water purification and ion transport due to their high porosity, clear pore structure, uniform and adjustable pore size, and adjustable pore properties. Covalent organic framework membranes can realize ordered one-dimensional nanochannels. Their high-density, regularly arranged nanochannels reduce the migration path of ion transport and can effectively reduce membrane resistance.
[0004] However, the crystallinity and mechanical strength of covalent organic framework membranes still need to be improved, and it is still difficult to prepare independent and easy-to-operate covalent organic framework membranes, which limits the practical application of covalent organic framework membranes. It is still challenging to develop large-scale nanofluid membranes with high flux, high charge density, and flexible self-support. In the face of the current bottleneck in the field of nanochannel membrane materials, it is still necessary to construct a flexible membrane material with regular and orderly structure and adjustable thickness to realize intelligent ion transport. Summary of the invention
[0005] The present invention aims to solve the bottleneck faced by current nanofluidic membrane devices, combines a GO / ANF membrane with good mechanical strength with a COF membrane with advantages such as high specific surface area, high charge density and ion conduction efficiency, and provides a COF / GO / ANF composite membrane and a preparation method thereof. The present invention uses an interfacial polymerization method to synthesize a covalent organic framework film connected by imine bonds, and transfers the film to a GO / ANF membrane prepared by a vacuum filtration method to form a self-supporting composite membrane with a regular and orderly structure and adjustable thickness. The composite membrane includes a covalent organic framework film with a high surface charge density of several hundred nanometers (400-800 nm) and a graphene oxide film containing aramid fibers with a thickness of about several micrometers (2-5 μm). The heterogeneous membrane has an asymmetric chemical composition and an asymmetric channel structure. The advantages of the two types of films are combined, giving the membrane considerable application prospects in the field of intelligent ion transport. The present invention provides a new idea for the preparation of new nanofluidic devices and solid-state nanochannel membranes. The strategy of combining one-dimensional microporous channels with two-dimensional sub-nano channels has considerable application prospects in intelligent ion transport.
[0006] The technical solution of the present invention is specifically described as follows.
[0007] The present invention provides a COF / GO / ANF composite nanochannel membrane, which is an upper and lower layer structure, and is composed of a covalent organic framework COF film layer with a one-dimensional microporous channel structure and a graphene oxide GO film layer containing aramid fiber ANF with a two-dimensional sub-nanometer channel structure; the membrane is prepared by the following steps: (1) Using trialdehyde phloroglucinol Tp as an aldehyde-containing monomer and 2,5-diaminobenzenesulfonic acid Pa-SO3H as an amine-containing monomer, a crystalline COF membrane was synthesized by a bottom-up method based on diffusion and solvent co-mediated polymerization at the organic phase / aqueous phase interface under the action of n-octanoic acid, and the crystalline COF membrane was immersed in deionized water for later use; (2) A GO / ANF membrane was prepared on a nylon filter membrane using a dispersion of GO and ANF by vacuum filtration, and then the GO / ANF membrane with the nylon filter membrane was dried to stabilize the GO / ANF membrane; (3) Using the dried GO / ANF membrane with a nylon filter membrane as the substrate, the crystalline COF membrane was transferred to the GO / ANF membrane. After drying in air, the nylon filter membrane was removed to obtain an independent, self-supporting flexible composite membrane.
[0008] The present invention also provides a method for preparing the above-mentioned COF / GO / ANF composite nanochannel membrane, and the specific steps are as follows: (1) Using trialdehyde phloroglucinol Tp as an aldehyde-containing monomer and 2,5-diaminobenzenesulfonic acid Pa-SO3H as an amine-containing monomer, a crystalline COF membrane was synthesized by a bottom-up method based on diffusion and solvent co-mediated polymerization at the organic phase / aqueous phase interface under the action of n-octanoic acid, and the crystalline COF membrane was immersed in deionized water for later use; (2) A GO / ANF membrane was prepared on a nylon filter membrane using a dispersion of GO and ANF by vacuum filtration, and then the GO / ANF membrane with the nylon filter membrane was dried to stabilize the GO / ANF membrane; (3) Using the GO / ANF membrane with a nylon filter membrane as the substrate, the crystalline COF membrane was transferred to the GO / ANF membrane. After drying in air, the nylon filter membrane was removed to obtain an independent, self-supporting flexible composite membrane.
[0009] In the present invention, step (1) is specifically as follows: The octanoic acid solution of the aldehyde-containing monomer Tp is added dropwise to the aqueous solution of the amine-containing monomer Pa-SO3H. After the addition, the mixture is placed in an oven at a temperature of 20-60°C and allowed to react for 24-120 hours. After the reaction is completed, the sample is taken out and washed to remove the unreacted monomer to obtain a crystalline COF membrane. The crystalline COF membrane is then immersed in deionized water for standby use. The molar ratio of the aldehyde-containing monomer Tp to the amine-containing monomer Pa-SO3H is 2:3. The concentration of the octanoic acid solution of the aldehyde-containing monomer Tp is 0.5-2.5 mg / mL, and the concentration of the aqueous solution of the amine-containing monomer Pa-SO3H is 0.5-2.5 mg / mL. During washing, N,N'-dimethylformamide DMF, ethanol and deionized water are used in sequence.
[0010] In the present invention, in step (1), an interfacial polymerization method is used to form a two-phase interface, and an organic phase is slowly dripped onto the aqueous phase to prevent excessive oscillation of the interface and rapid reaction of the monomer at the interface; the concentration of the monomer has a significant effect on the speed and thickness of the COF film formation, and the concentration of the reaction monomer in both phases should not be too high, so as to avoid too fast COF formation speed, accumulation of particles on the surface and unevenness, and a high concentration of the reaction monomer will also increase the thickness of the COF film, thereby affecting the tightness of the subsequent COF film and GO / ANF film bonding; the reaction temperature also has a certain effect on the growth rate and thickness of the COF film, and the reaction temperature should not be too high, so as to avoid too fast reaction speed and rough and uneven COF film surface; the reaction time has a certain effect on the crystallinity of the COF film, and if the reaction time is too short, the COF crystallinity is not high.
[0011] In the present invention, in step (2), in the dispersion of GO and ANF, the mass ratio of GO to ANF is 5:1-8:1, and the solvent is a mixed solvent of dimethyl sulfoxide (DMSO) and water in a volume ratio of 30:1-50:1.
[0012] In the present invention, the dispersion of GO and ANF is prepared by the following method: Firstly, graphene oxide GO nanosheets are dispersed in DMSO and ultrasonicated until uniformly dispersed to obtain a graphene oxide GO dispersion with a concentration of 0.5-1.5 mg / mL; after adding Kevlar yarn and KOH into DMSO, stirring at a temperature of 35-45°C until completely dissolved, an aramid nanofiber ANF dispersion with a concentration of 1-3 mg / mL is obtained; the graphene oxide GO nanosheets use single-layer graphene oxide powder with a sheet diameter of 0.5-5 μm and a thickness of 0.8-1.2 nm; Then, the GO dispersion and ANF dispersion were mixed and ultrasonically treated for 15-25 min; Then, DMSO with a volume of 2-4 times the volume of GO dispersion was added to the system, and ultrasonication was continued for 10-20 min to better disperse ANF and GO in DMSO. Finally, deionized water was added to the system and ultrasonicated for 20 min to 40 min to deprotonate and form a homogeneous suspension.
[0013] In the present invention, in step (2), during vacuum filtration, the average pore size of the nylon filter membrane is 0.2 μm, and the pressure is between 0.08-0.12 MPa; after vacuum filtration, the GO / ANF membrane with the nylon filter membrane is first placed in the air to dry (natural drying), and then placed in an oven at 75-85°C for 20-30 h. The vacuum filtration time is related to the volume of the filtered dispersion. You can continue to filter for five minutes after there is no obvious liquid on the surface and then stop.
[0014] In the present invention, in step (3), based on the evaporation-induced self-assembly strategy, the GO / ANF membrane with a nylon filter membrane is used as the substrate, and the COF membrane is evenly attached to the GO / ANF membrane. As the water evaporates, the composite membrane is gradually separated from the underlying filter membrane to obtain a self-supporting membrane.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention combines the COF membrane formed by interfacial polymerization with the GO / ANF membrane prepared by vacuum filtration through an interfacial superassembly strategy to obtain a composite nanochannel membrane. The composite membrane has rich surface groups, asymmetric chemical composition and asymmetric channel structure. The advantages of the two types of films are combined, giving the composite membrane considerable application prospects in the field of intelligent ion transmission, and at the same time providing reference significance for the construction of nanofluidic reverse osmosis system.
[0016] The COF / GO / ANF membrane prepared by the present invention includes a COF membrane with a negative charge on the surface and a negatively charged GO / ANF membrane containing a certain mass of ANF. Compared with other nanochannel membranes, the composite membrane has higher mechanical stability and surface charge density, and a regular and orderly pore structure. These advantages greatly reduce the internal resistance of ion transmission, which is conducive to the application of the composite membrane in intelligent ion transmission. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a preparation flow chart of the present invention based on the interface superassembly strategy.
[0018] Figure 2 : (a), (b) and (c) are transmission electron microscopy (TEM) images of the COF films prepared in Examples 1, 2 and 3, respectively.
[0019] Figure 3 3 are scanning electron microscope (SEM) images of the surface COF side (a), the surface GO / ANF side (b) and the cross section (c) of the COF / GO / ANF composite membrane prepared in Example 1 of the present invention.
[0020] Figure 4 : These are Fourier transform infrared spectra of the COF film (TpPa-SO3H) (a) and the GO / ANF film (b) of Example 1 of the present invention.
[0021] Figure 5 1 and 2. The small-angle X-ray scattering pattern of the COF film prepared in Example 1 of the present invention (a) and the X-ray diffraction pattern of the GO / ANF film (b).
[0022] Figure 6 3 and 4. These are contact angle test diagrams of the COF membrane side (a) and the GO / ANF membrane side (b) of the COF / GO / ANF composite membrane prepared in Example 1 of the present invention.
[0023] Figure 7 It is a stress-strain curve diagram of the COF / GO / ANF composite film prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] In order to explain the present invention in more detail, the present invention is described in detail below with reference to examples and drawings. The present invention first uses a bottom-up method to synthesize a COF membrane at the interface of two phases (organic phase / aqueous phase) through diffusion and solvent co-mediation, and then uses vacuum filtration to prepare an ultra-thin GO / ANF membrane on a nylon filter membrane. With the GO / ANF membrane as the substrate, the COF membrane is transferred to the GO / ANF membrane, and after drying in air, an independent self-supporting flexible composite membrane can be obtained, which provides abundant nanochannels for ion transport. Specific examples are as follows. Example 1
[0025] The preparation method of the COF / GO / ANF composite membrane specifically comprises the following steps: Step 1: Add 21.0 mg of trialdehyde phloroglucinol (Tp) to 20 mL of octanoic acid and sonicate for 15 min until completely dissolved; Step 2: Add 28.2 mg of 2,5-diaminobenzenesulfonic acid (Pa-SO3H) to 30 mL of deionized water and sonicate for 15 min until completely dissolved; Step 3: slowly drop the octanoic acid containing aldehyde monomer Tp into the upper layer of the aqueous solution containing amine monomer Pa-SO3H, and place it in a 30°C oven to react for 3 days; Step 4: washing the synthesized COF film with DMF, ethanol and deionized water in sequence to remove unreacted monomers; Step 5: Soak the washed COF membrane in deionized water for subsequent operation; Step 6: 1.0 g of Kevlar yarn and 1.5 g of KOH were added to 500 mL of DMSO, and the mixture was stirred at 40 °C for 10 days until completely dissolved, resulting in a dark red aramid nanofiber (ANF) dispersion (2 mg / mL); Step 7: Disperse 0.1 g of graphene oxide (GO) nanosheets in 100 mL of DMSO and sonicate for 1 h until uniformly dispersed to obtain a GO dispersion (1 mg / mL); Step 8: Take 0.75 mL of ANF dispersion (2 mg / mL), add it to 10 mL of GO dispersion (1 mg / mL) in DMSO, and sonicate for 20 min. Step 9: Add 30 mL of DMSO to the above mixture and sonicate for 15 min to better disperse the ANF in the DMSO solution of GO; Step 10: Add 1 mL of deionized water to the above mixture and sonicate for 0.5 h to deprotonate and form a homogenous suspension; Step 11: The GO / ANF mixture was vacuum filtered on a nylon filter membrane (47 mm, 0.2 μm); Step 12: After filtration, remove the filter membrane, place it in the air to dry, and then heat it in an oven at 80°C for 24 hours to stabilize the membrane; Step 13: Carefully transfer the synthesized COF film soaked in deionized water to the GO / ANF membrane, and dry the composite membrane in air. After drying, the COF / GO / ANF composite membrane can be peeled off from the nylon filter membrane to obtain a self-supporting membrane. Example 2
[0026] The preparation method of the COF / GO / ANF composite membrane specifically comprises the following steps: Step 1: Add 21.0 mg of trialdehyde phloroglucinol (Tp) to 20 mL of octanoic acid and sonicate for 15 min until completely dissolved; Step 2: Add 28.2 mg of 2,5-diaminobenzenesulfonic acid (Pa-SO3H) to 30 mL of deionized water and sonicate for 15 min until completely dissolved; Step 3: slowly drop the octanoic acid containing aldehyde monomer Tp into the upper layer of the aqueous solution containing amine monomer Pa-SO3H, and place it in a 60°C oven to react for 3 days; Step 4: washing the synthesized COF film with DMF, ethanol and deionized water in sequence to remove unreacted monomers; Step 5: Soak the washed COF membrane in deionized water for subsequent operation; Step 6: 1.0 g of Kevlar yarn and 1.5 g of KOH were added to 500 mL of DMSO, and the mixture was stirred at 40 °C for 10 days until completely dissolved, resulting in a dark red aramid nanofiber (ANF) dispersion (2 mg / mL); Step 7: Disperse 0.1 g of graphene oxide (GO) nanosheets in 100 mL of DMSO and sonicate for 1 h until uniformly dispersed to obtain a GO dispersion (1 mg / mL); Step 8: Take 0.75 mL of ANF dispersion (2 mg / mL), add it to 10 mL of GO dispersion (1 mg / mL) in DMSO, and sonicate for 20 min. Step 9: Add 30 mL of DMSO to the above mixture and sonicate for 15 min to better disperse the ANF in the DMSO solution of GO; Step 10: Add 1 mL of deionized water to the above mixture and sonicate for 0.5 h to deprotonate and form a homogenous suspension; Step 11: The GO / ANF mixture was vacuum filtered on a nylon filter membrane (47 mm, 0.2 μm); Step 12: After filtration, remove the filter membrane, place it in the air to dry, and then heat it in an oven at 80°C for 24 hours to stabilize the membrane; Step 13: Carefully transfer the synthesized COF film soaked in deionized water to the GO / ANF membrane, and dry the composite membrane in air. After drying, the COF / GO / ANF composite membrane can be peeled off from the nylon filter membrane to obtain a self-supporting membrane. Example 3
[0027] The preparation method of the COF / GO / ANF composite membrane specifically comprises the following steps: Step 1: Add 42.0 mg of trialdehyde phloroglucinol (Tp) to 20 mL of n-octanoic acid and sonicate for 15 min until completely dissolved; Step 2: Add 56.4 mg of 2,5-diaminobenzenesulfonic acid (Pa-SO3H) to 30 mL of deionized water and sonicate for 15 min until completely dissolved; Step 3: slowly drop the octanoic acid containing aldehyde monomer Tp into the upper layer of the aqueous solution containing amine monomer Pa-SO3H, and place it in a 30°C oven to react for 3 days; Step 4: washing the synthesized COF film with DMF, ethanol and deionized water in sequence to remove unreacted monomers; Step 5: Soak the washed COF membrane in deionized water for subsequent operation; Step 6: 1.0 g of Kevlar yarn and 1.5 g of KOH were added to 500 mL of DMSO, and the mixture was stirred at 40 °C for 10 days until completely dissolved, resulting in a dark red aramid nanofiber (ANF) dispersion (2 mg / mL); Step 7: Disperse 0.1 g of graphene oxide (GO) nanosheets in 100 mL of DMSO and sonicate for 1 h until uniformly dispersed to obtain a GO dispersion (1 mg / mL); Step 8: Take 0.75 mL of ANF dispersion (2 mg / mL), add it to 10 mL of GO dispersion (1 mg / mL) in DMSO, and sonicate for 20 min. Step 9: Add 30 mL of DMSO to the above mixture and sonicate for 15 min to better disperse the ANF in the DMSO solution of GO; Step 10: Add 1 mL of deionized water to the above mixture and sonicate for 0.5 h to deprotonate and form a homogenous suspension; Step 11: The GO / ANF mixture was vacuum filtered on a nylon filter membrane (47 mm, 0.2 μm); Step 12: After filtration, remove the filter membrane, place it in the air to dry, and then heat it in an oven at 80°C for 24 hours to stabilize the membrane; Step 13: Carefully transfer the synthesized COF film soaked in deionized water to the GO / ANF membrane, and dry the composite membrane in air. After drying, the COF / GO / ANF composite membrane can be peeled off from the nylon filter membrane to obtain a self-supporting membrane.
[0028] Figure 1 This is a flow chart for preparing the COF / GO / ANF composite membrane of Example 1. Figure 2 This is a transmission electron microscope image of the COF film. Figure 2 a, 2b and 2c correspond to the COF films prepared in Examples 1, 2 and 3, respectively. Clear lattice fringes can be seen from the TEM images, indicating that the COF film has good crystallinity and relatively ordered pores. Figure 3 This is a scanning electron microscope image of the COF / GO / ANF composite membrane. Figure 3 a and 3b are the surfaces of the composite membrane prepared in Example 1, Figure 3 a is the COF side of the composite membrane, Figure 3 b is the GO / ANF side of the composite membrane. It can be seen that the membrane surface is relatively flat without obvious defects. Figure 3 c is the cross-section of the COF / GO / ANF composite membrane, where we can see the relatively compact COF membrane with a thickness of several hundred nanometers on the upper layer and the layered GO / ANF membrane on the lower layer. Figure 4The Fourier transform infrared spectra of the COF membrane (TpPa-SO3H) and GO / ANF membrane prepared in Example 1 show that Figure 4 The TpPa-SO3H COF membrane synthesized in a does not contain the amino and aldehyde groups in the reactive monomers, but generates imine bonds, indicating that the COF membrane was successfully synthesized without any reactive monomer residues. Figure 4 The GO / ANF film in b also contains the corresponding characteristic groups, indicating that ANF is successfully assembled into GO. Figure 5 is a small angle X-ray scattering diagram of the COF film prepared in Example 1 of the present invention and an X-ray diffraction diagram of the GO / ANF film, Figure 5 The COF film in a has an obvious peak at 5°, corresponding to the (100) crystal plane, indicating that the COF has good crystallinity. Figure 5 The XRD peaks of GO film and GO / ANF film in b are located at 10.0° and 10.7°, respectively, indicating that the introduction of ANF can change the interlayer spacing and improve the interfacial connection between graphene oxide nanosheets, which is conducive to better ion transport. Figure 6 is the contact angle test result of the COF film side and the GO / ANF film side of the COF / GO / ANF composite film prepared in Example 1 of the present invention, Figure 6 The contact angle of the COF film in a is 9.38 ± 0.10°. Figure 6 The contact angle of the GO / ANF membrane in b is 56.29 ± 0.18°. It can be seen that the COF membrane is more hydrophilic than the GO / ANF membrane, and there are abundant hydrophilic groups on the surface of the COF membrane. Figure 7 : is the stress-strain curve of the COF / GO / ANF composite membrane prepared in Example 1 of the present invention, and it can be seen that the composite membrane has high mechanical strength. These results reflect the successful construction of the COF / GO / ANF composite membrane.
[0029] As described above, the COF / GO / ANF composite membrane with regular structure and adjustable thickness prepared by the interface superassembly strategy of the present invention provides a new material for nanofluidic membrane devices in the field of intelligent ion transport.
Claims
1. A COF / GO / ANF composite nanochannel membrane, characterized in that: It is a top-bottom structure, consisting of a covalent organic framework COF film layer with a one-dimensional microporous channel structure and a graphene oxide GO film layer containing aramid fiber ANF with a two-dimensional sub-nano channel structure; It is prepared by the following steps: (1) Using trialdehyde phloroglucinol Tp as an aldehyde-containing monomer and 2,5-diaminobenzenesulfonic acid Pa-SO3H as an amine-containing monomer, a crystalline COF membrane was synthesized by a bottom-up method based on diffusion and solvent co-mediated polymerization at the organic phase / aqueous phase interface under the action of n-octanoic acid, and the crystalline COF membrane was immersed in deionized water for later use; (2) A GO / ANF membrane was prepared on a nylon filter membrane using a dispersion of GO and ANF by vacuum filtration, and then the GO / ANF membrane with the nylon filter membrane was dried to stabilize the GO / ANF membrane; (3) Using the dried GO / ANF membrane with a nylon filter membrane as the substrate, the crystalline COF membrane was transferred to the GO / ANF membrane. After drying in air, the nylon filter membrane was removed to obtain an independent, self-supporting flexible composite membrane.
2. A method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 1, characterized in that: The specific steps are as follows: (1) Using trialdehyde phloroglucinol Tp as an aldehyde-containing monomer and 2,5-diaminobenzenesulfonic acid Pa-SO3H as an amine-containing monomer, a crystalline COF membrane was synthesized by a bottom-up method based on diffusion and solvent co-mediated polymerization at the organic phase / aqueous phase interface under the action of n-octanoic acid, and the crystalline COF membrane was immersed in deionized water for later use; (2) A GO / ANF membrane was prepared on a nylon filter membrane using a dispersion of GO and ANF by vacuum filtration, and then the GO / ANF membrane with the nylon filter membrane was dried to stabilize the GO / ANF membrane; (3) Using the GO / ANF membrane with a nylon filter membrane as the substrate, the crystalline COF membrane was transferred to the GO / ANF membrane. After drying in air, the nylon filter membrane was removed to obtain an independent, self-supporting flexible composite membrane.
3. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 2, characterized in that: Step (1) is as follows: The n-octanoic acid solution of the aldehyde-containing monomer Tp is added dropwise to the aqueous solution of the amine-containing monomer Pa-SO3H. After the addition, the mixture is placed in an oven at a temperature of 20-60°C and allowed to react for 24-120 hours. After the reaction is completed, the sample is taken out and washed to remove the unreacted monomer to obtain a crystalline COF membrane. The crystalline COF membrane is then immersed in deionized water for standby use. The molar ratio of the aldehyde-containing monomer Tp to the amine-containing monomer Pa-SO3H is 2:
3.
4. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 3, characterized in that: The concentration of the octanoic acid solution containing the aldehyde monomer Tp is 0.5-2.5 mg / mL, and the concentration of the aqueous solution containing the amine monomer Pa-SO3H is 0.5-2.5 mg / mL.
5. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 3, characterized in that: During washing, N,N'-dimethylformamide DMF, ethanol and deionized water are used in sequence.
6. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 2, characterized in that: In step (2), in the dispersion of GO and ANF, the mass ratio of GO to ANF is 5:1-8:1, and the solvent is a mixed solvent of dimethyl sulfoxide (DMSO) and water in a volume ratio of 30:1-50:
1.
7. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 6, characterized in that: The dispersions of GO and ANF were prepared by the following method: First, graphene oxide GO nanosheets are dispersed in DMSO and ultrasonicated until uniformly dispersed to obtain a graphene oxide GO dispersion with a concentration of 0.5-1.5 mg / mL; after Kevlar yarn and KOH are added to DMSO, they are stirred at a temperature of 35-45°C until completely dissolved to obtain an aramid nanofiber ANF dispersion with a concentration of 1-3 mg / mL; Then, the GO dispersion and ANF dispersion were mixed and ultrasonically treated for 15-25 min; Then, DMSO with a volume of 2-4 times the volume of the GO dispersion was added, and ultrasonication was continued for 10-20 min to better disperse the ANF and GO in the DMSO. Finally, deionized water was added and ultrasonicated for 20 min to 40 min to deprotonate and form a homogeneous suspension.
8. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 7, characterized in that: Graphene oxide GO nanosheets are made of single-layer graphene oxide powder with a sheet diameter of 0.5-5 μm and a thickness of 0.8-1.2 nm.
9. The method for preparing the COF / GO / ANF composite nanochannel membrane according to claim 2, characterized in that: In step (2), during vacuum filtration, the average pore size of the nylon filter membrane is 0.2 μm, and the pressure is between 0.08-0.12 MPa; after vacuum filtration, the GO / ANF membrane with the nylon filter membrane is first placed in the air to dry, and then placed in an oven at 75-85°C and heated for 20-30 h.
Citation Information
Cited By
Application of photoresponse asymmetric nanofluid film in reverse electrodialysis power generation
CN119656870A
Application of a photoresponsive asymmetric nanofluid membrane in reverse electrodialysis power generation
CN119656870B