Preparation method of low-temperature catalytic oxidation catalyst and application of low-temperature catalytic oxidation catalyst in dealdehyding reaction
By preparing low-temperature catalytic oxidation catalysts on common oxide support, the problems of high cost and high-temperature reduction processes of precious metals are solved, and the effect of efficient formaldehyde removal at room temperature is achieved.
Patent Information
- Application Number
- CN202411182975.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
The existing dealdehyde catalysts have high cost and high temperature reduction processes such as precious metal Pt, which leads to high production costs and poor formaldehyde removal efficiency at room temperature.
The surface modification is performed on commonly used oxide support by using a three-step impregnation method, and low-cost first and second surface modification agents are used, combined with active components such as Ag2O to form a low-temperature catalytic oxidation catalyst to achieve efficient removal of formaldehyde at room temperature.
It achieves efficient oxidation of formaldehyde into CO2 and water at low temperatures, reducing the production cost of the catalyst, is suitable for large-scale production and application, and has high catalyst activity and long life, and is suitable for indoor removal of low-concentration formaldehyde.
Smart Images

Figure CN118988283A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aldehyde removal catalysts, and particularly relates to a preparation method of a low-temperature catalytic oxidation catalyst and application of the catalyst in aldehyde removal reactions. Background Art
[0002] Formaldehyde is an important precursor for the synthesis of many other materials and compounds. Millions of tons of formaldehyde are consumed each year and are widely used in the manufacture of various building materials and household products. Particleboard, plywood and fiberboard are the main sources of formaldehyde in indoor air. The impact of formaldehyde on human health is mainly manifested in irritation to the respiratory system. Long-term exposure can also cause abnormal liver function and immune system, induce gene mutations, and increase the incidence of cancer. Therefore, the removal of formaldehyde in indoor air is of great research significance.
[0003] At present, the main methods for removing formaldehyde include adsorption, thermal catalytic oxidation, photocatalytic oxidation, plasma technology, etc. Adsorption is the simplest method, with fast removal, high efficiency and low cost. However, it is limited by the limited adsorption capacity of the adsorbent. Thermal catalytic oxidation can continuously and completely decompose HCHO into harmless H2O and CO2, but it is limited by the catalyst. It is difficult for non-precious metal catalysts to completely convert formaldehyde into CO2 and H2O at room temperature. Although precious metals are more active at room temperature, they are expensive and difficult to use in large quantities. The photocatalyst itself is non-toxic and harmless, has high stability, does not require too much energy for the reaction, and the reaction products are clean and harmless, but requires reliable light source production equipment. The common photocatalyst TiO2 is more active under ultraviolet light, but the response is not high under visible light. Ultraviolet light only accounts for 5% of the solar spectrum, and visible light accounts for about 43%, so the utilization rate of light by the photocatalyst TiO2 is very low. Plasma decomposition of formaldehyde takes a short time, has a large processing capacity, a high decomposition efficiency, and can be carried out at room temperature and pressure, but it may produce harmful byproducts such as ozone and nitrogen oxides.
[0004] In recent years, studies have shown that precious metals such as Pt, Pd, and Au have high activity against formaldehyde at low temperatures. CN115301231A discloses a method for preparing a catalyst for removing formaldehyde loaded with precious metal Pt. Using γ-Al2O3 as a carrier to load 0.03-0.05wt.% Pt and 1wt.% Na, at 25°C, the removal rate of 110 ppm of formaldehyde within 6 hours is 100%. The catalyst preparation requires that pseudo-boehmite powder be calcined at 200-350°C for 2-3h, then heated to 450-550°C and calcined for 3-4h to obtain carrier Al2O3; then rotary evaporation at 40-80°C, drying at 60-100°C for 1-12h, and calcination at 200-400°C for 2-3h to obtain additive / Al2O3; noble metal salt and additive / Al2O3 aqueous solution are mixed and stirred, then rotary evaporation at 40-80°C, drying at 60-100°C for 1-12h, calcination at 500-700°C for 3-4h, and reduction at 300-500°C in a hydrogen atmosphere for 30-360min to obtain the noble metal catalyst. Although the catalyst prepared by this method can completely convert formaldehyde at room temperature, the cost of loading the noble metal is relatively high, and the catalyst preparation process is extremely complicated, especially the high-temperature hydrogen reduction process is required, so that the production cost is relatively high. In addition, the catalyst takes a long time to remove formaldehyde and is not suitable for indoor formaldehyde removal applications.
[0005] It is reported that silver (Ag)-based catalysts also have good activity in catalytic oxidation reactions, and the price of silver is only 1 / 100-1 / 40 of the price of precious metal Pt, which is much lower than the price of precious metal Pt. Therefore, silver-based de-aldehyde catalysts have received widespread attention. S. Imamura et al. prepared Ag / CeO2 catalysts by coprecipitation method. Ag can be highly dispersed on CeO2 and achieve 100% formaldehyde conversion rate at 200 ℃; L. Yu et al. synthesized CeO2 of different shapes by hydrothermal method, and then prepared Ag / CeO2 catalysts by loading Ag by impregnation method. CeO2 in the shape of nanorods loaded with Ag achieved a nearly 100% formaldehyde conversion rate at 100 ℃. L. Ma et al. prepared Ag / CeO2 nanosphere catalysts by one-step hydrothermal method. The test results showed that Ag / CeO2 nanosphere catalysts can completely convert formaldehyde into CO2 at temperatures above 110 ℃. These documents explored the feasibility of Ag-based catalysts, but also showed that the de-aldehyde effect of Ag catalysts was not as good as that of precious metal Pt catalysts. The reaction still required a relatively high temperature and could not achieve efficient conversion of formaldehyde at room temperature. At a relatively low temperature of 60-100 °C, only about 50% conversion rate could be achieved. In addition, the preparation processes and catalytic materials involved in the above documents are difficult or even impossible to put into industrial application.
[0006] In the field of patents, CN110548508A discloses the use of an oxidized non-platinum group metallizing agent in the catalytic oxidation of formaldehyde: the metal precursor is first impregnated on the carrier, and then the obtained solid is dried and calcined to prepare an oxidized metal catalyst. The oxidized metal precursor salt is selected from one or more combinations of AgNO3, CuSO4·5H2O, Fe(NO3)2·9H2O or NiCl2·6H2O. The carrier is one or more combinations of CeO2, La-CeO2, V-CeO2, Zr-CeO2, Ta-CeO2, Ca-CeO2 or Mn-CeO2. The Ag / La-CeO2 catalyst prepared by this method can achieve a formaldehyde conversion rate of 25% at 60 °C, but the Ag loading is relatively high, at 5wt.%. For Ag / CeO2 catalyst with Ag loading of 10wt.%, a conversion rate of 19% can be achieved at 60℃, while the conversion temperature of 50% is 80℃. The CeO2-based carrier used in this method needs to be homemade. Even if it can be mass-produced, the cost of CeO2 will be much higher than that of conventional catalyst carriers (such as Al2O3, SiO2), so the application prospects of CeO2 as a carrier are worrying. In addition, the ability of this catalyst to remove low concentrations of formaldehyde (such as 1 ppm and below) in actual scenarios is unknown. Summary of the invention
[0007] In view of the technical problems in the prior art of formaldehyde removal catalysts, such as the large amount of high-cost transition metal oxides such as CeO2 used or the active ingredients using expensive precious metals such as Pt, which leads to high catalyst preparation costs and thus limits their applications, the present invention has developed a method for preparing a low-temperature catalytic oxidation catalyst. The catalyst does not require the use of precious metals such as Pt, and the amount of active metal used is low. It can have higher activity and lower cost at low temperatures. It is used for formaldehyde removal reactions. At a low active metal content (≤2wt.%), formaldehyde can be completely oxidized into carbon dioxide and water at low temperatures (not higher than 100°C, more preferably not higher than 85°C). The catalyst has high activity, low manufacturing cost, long life, stable performance, and is suitable for large-scale production and application.
[0008] The technical solution of the present invention is as follows: A method for preparing a low-temperature catalytic oxidation catalyst adopts a three-step impregnation method to impregnate a first surface modifier, a second surface modifier and a catalyst active component on a catalyst carrier respectively. The catalyst carrier adopts a commonly used and inexpensive oxide carrier, such as SiO2 and gamma alumina (g-Al2O3). The first surface modifier can spread on the surface of the catalyst carrier, change the surface properties of the original oxide carrier, make the cheap carrier show the surface properties of the first surface modifier, and continue to maintain the original carrier strength in terms of mechanical strength. The second surface modifier is rich in oxygen vacancies and is used to enhance the low-temperature activity of the catalyst. If the composite oxides Cr2O3-TiO2 and La2O3-CeO2 rich in oxygen vacancies and able to spread are directly used to modify the carrier surface, it is also possible to perform surface modification only once.
[0009] Furthermore, the catalyst carrier is required to have a high specific surface area and a large pore size. For example, the more widely used gamma alumina (g-Al2O3), silicon oxide (SiO2) and activated carbon all have a high specific surface area, but activated carbon is not suitable for subsequent high-temperature calcination and is not considered; other composite carriers include SiO2-Al2O3, molecular sieves, calcined hydrotalcite, etc. These catalysts are widely used and are cheap and easy to obtain.
[0010] Furthermore, the first surface modifier is a transition metal oxide. The first surface modifier can spread efficiently on the catalyst carrier and promote the growth of the second surface modifier on its surface. The first surface modifier spreads on the surface of the catalyst carrier, changes or even determines the surface properties of the carrier, and is preferably a metal oxide with the same metal valence state and different metal elements as the catalyst carrier. If Al2O3 is used as a catalyst carrier, the first surface modifier selected is a trivalent transition metal oxide whose metal element is not Al, mainly a trivalent metal oxide of the third group of the periodic table, such as Sc2O3, Y2O3, La2O3; or a trivalent metal oxide of the 13th group of the periodic table, such as Ga2O3, In2O3; or a trivalent compound of a transition metal in the third row of the periodic table, such as Cr2O3, Fe2O3. Because of the similarity of the lattice, these trivalent metal oxides are easy to spread on the Al2O3 surface. If SiO2 is used as the carrier, the first surface modifier needs to be a tetravalent transition metal oxide whose metal element is not Si, including TiO2, ZrO2, MnO2, MoO2, and SnO2 of Group XIV.
[0011] Furthermore, the second surface modifier is coated on the surface of the first surface modifier in the form of a thin film, so that the low-cost catalyst carrier exhibits the function of a high-performance and high-cost carrier. The second surface modifier is a transition metal oxide rich in oxygen vacancies, including metal oxides CuO, ZnO, CeO2, ZrO2, TiO2, WO3, MoO3, etc. This part of the components is used to provide a high-performance carrier surface. In order to introduce more oxygen vacancies, low-valent doped metal oxides can also be introduced into the above-mentioned metal oxides at the same time. The low-valent state means that the valence of the doped metal is lower than the one or two valences of the doped metal, such as introducing Cu2O into ZnO; introducing La2O3 or Y2O3 into CeO2; introducing Y2O3 into ZrO2; introducing V2O5 or MnO2 into WO3 and MoO3, etc. The schematic diagram of oxygen vacancies is shown in the figure below. Figure 1 As shown, the formation of oxygen vacancies is used to anchor the oxygen atoms in formaldehyde and promote the formaldehyde oxidation reaction.
[0012] Furthermore, the second surface modifier contains at least one component that is the same as the oxide in the first surface modifier, so that the second surface modifier can spread on the surface of the first surface modifier. For example, when the first surface modifier is Cr2O3, the second surface modifier can be CuO-Cr2O3, Cr2O3-TiO2 (the latter oxide has a higher mass ratio), etc.; when the first surface modifier is La2O3, the second surface modifier can be BaO-La2O3, La2O3-CeO2, etc.
[0013] In particular, when the second surface modifier can be spread on the surface of the catalyst carrier, only the second surface modifier can be used, and the first impregnation and the first surface modifier can be omitted. For example, Al2O3 is used as the carrier, La2O3 is used as the first surface modifier, and La2O3-CeO2 is used as the second surface modifier. Since La2O3-CeO2 can exhibit the characteristics of La2O3 even when the mass fraction of CeO2 in the composite reaches more than 90%, La2O3-CeO2 can also be spread directly on the surface of the Al2O3 carrier, that is, it can play the role of the first and second surface modifiers at the same time.
[0014] Furthermore, the catalyst active components include main catalyst Ag2O, Cu2O, FeO, Co3O4, NiO and MnO x At least one of the above, and at least one of the corresponding oxides of the co-catalysts Li, Na, K, and Cs, the co-catalyst being used to enhance the separation of the generated CO2.
[0015] Furthermore, in the first and second surface modifier impregnations, the metal oxide precursors used are nitrates, sulfates, chlorides, acetates, and oxalates corresponding to the metal oxides. After drying and calcination, a catalyst carrier with a surface modifier is obtained. After a second impregnation-drying-calcination, a surface-modified carrier is obtained. The surface-modified carrier is then impregnated with an active component for the third time. The solution used is a nitrate, sulfate, acetate, oxalate or chloride (except silver) solution of the metal corresponding to the active component. After drying and calcination again, the catalyst product is obtained.
[0016] Furthermore, in the obtained catalyst, the carrier mass accounts for 80-90wt%, the first and second surface modifiers account for 7-19wt% in total, and the active component accounts for 1-3wt%. Because the mass proportion of the surface modifier and the catalyst active component is very small, the preparation process only uses impregnation and calcination, so the catalyst prepared by this method has low cost.
[0017] The above catalyst is used for the dealdehyde reaction and has the ability to catalyze the oxidation of formaldehyde at room temperature (25°C), and this ability becomes stronger as the temperature increases. At above 85°C, the catalyst can convert about 100 ppm of formaldehyde into CO2 and water, and the required residence time is 0.17 seconds.
[0018] The present invention obtains a dealdehyde catalyst with excellent performance by modifying the surface of a common catalyst carrier to be rich in oxygen vacancies and then loading the active metal component thereon. By utilizing the spreading effect, the surface of the cheap catalyst carrier is covered with a layer of different metal oxide layers, thereby showing the performance of the covering layer to the outside. This covering layer can use more expensive or rare metal oxides, which has an effect similar to that of good steel placed on a knife edge. For example, La2O3 can be spread on Al2O3, Y2O3 can also be spread; TiO2 can be spread on SiO2. After a small amount of other elements are doped between La2O3, Y2O3 and TiO2, their spreading on the corresponding catalyst carrier is not affected. At the same time, because of this spreading effect, oxygen vacancies are constructed, the low-temperature activity of the catalyst is improved, so that a small amount of relatively cheap catalysts (such as silver-based catalysts) can achieve the catalytic effect that can only be achieved by precious metal catalysts such as gold and palladium.
[0019] In addition, since the carrier can directly use commercial catalyst carriers instead of various homemade nanocatalyst carriers, the catalyst production has industrial application feasibility. The overall preparation method is simple and does not require expensive catalyst preparation routes such as hydrogen atmosphere reduction.
[0020] The beneficial effects of the present invention are: Compared with the existing process, the preparation method of the formaldehyde removal catalyst involved in the present invention is relatively simple. No precious metal catalysts such as Pt are used. The oxygen vacancy theory is used to modify the surface of the traditional carrier, thereby greatly improving the catalytic oxidation performance of the active components of the catalyst without significantly increasing the production cost, so that the catalyst can obtain a formaldehyde conversion rate of nearly 100% at close to room temperature or lower temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of oxygen vacancies.
[0022] Figure 2 XRD patterns of Al2O3 and Y2O3-La / Al2O3 catalysts in Example 1.
[0023] Figure 3 This is the XRD spectrum of SiO2 and TiO2 / SiO2 catalysts in Example 2.
[0024] Figure 4 XRD patterns of Al2O3 and CeO2-La / Al2O3 catalysts in Example 3.
[0025] Figure 5 XRD spectra of Al2O3 and CeO2-La / Al2O3 catalysts of Example 4.
[0026] Figure 6 This is the XRD spectrum of SiO2 and Cr2O3-TiO2 / SiO2 catalyst in Example 5.
[0027] Figure 7 XRD patterns of SiO2 and Cr2O3-TiO2 / SiO2 catalysts of Example 6.
[0028] Figure 8 The dealdehyde conversion rate of the Ag / TiO2-Cr2O3 / SiO2 catalyst in Example 7 at different temperatures.
[0029] Fig. 9 The dealdehyde conversion rates of the catalysts with different Cr contents in Example 8 at different temperatures.
[0030] Fig.10 The dealdehyde conversion rates of the catalysts with different La contents in Example 9 at different temperatures.
[0031] Fig.11 The dealdehyde conversion rate of different impregnation AgNO3 solution concentrations in Example 11.
[0032] Fig.12 The effect of co-catalysts Na and K on the dealdehyde conversion rate.
[0033] Fig.13 A comparison of Pt catalyst and Ag catalyst of equal value.
[0034] Fig.14 Comparison of the dealdehyde performance of Cu catalyst and Ag catalyst.
[0035] Fig.15 Comparison of the dealdehyde performance of Co catalyst and Ag catalyst.
[0036] Fig.16 Comparison of the dealdehyde performance of Ag catalysts at different concentrations.
[0037] Fig.17 The effect of catalyst modifiers on the dealdehyde performance at different temperatures.
[0038] Fig.18 Comparison of the adsorption performance of catalysts under different atmospheres. DETAILED DESCRIPTION
[0039] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited thereto.
[0040] Example 1 Spreading Example of the First Surface Modifier on the Surface of Al2O3 Support Yttrium nitrate (0.5 mol / L) and lanthanum nitrate solution (0.5 mol / L) were impregnated on the catalyst carrier Al2O3, dried and calcined at 450 ℃. Figure 2 The XRD spectrum shown in the figure did not observe the peaks of Y2O3 and La2O3. The lattice size of Al2O3 increased from 2.3 nm to 2.5 nm and 2.6 nm respectively. The BET data showed that the pore volume and pore size of Al2O3 were significantly reduced. The pore volume of Al2O3 increased from 0.8 cm 3 / g decreased to 0.69 and 0.64 cm 3 Both XRD and BET data show that Y2O3 and La2O3 spread on the pore surface inside Al2O3 instead of forming particles.
[0041] Example 2 Spreading of the first surface modifier on the surface of the SiO2 carrier A mixed solution of titanyl sulfate (0.5 mol / L) and sulfuric acid (0.1 mol / L) was impregnated on the catalyst carrier SiO2, dried and then calcined at 600°C. Figure 3 The XRD spectrum shown in the figure did not show any peaks of TiO2. The lattice size of SiO2 was 3.4 nm, and no significant changes were observed. However, the BET data showed that the pore volume of SiO2 was significantly reduced from 0.8 cm 3 / g dropped to 0.64cm 3 / g. XRD and BET data show that TiO2 spreads on the pore surface inside SiO2 instead of forming particles.
[0042] Example 3 Loading the second surface modifier La2O3-CeO2 on the Al2O3 carrier The La2O3-modified Al2O3 catalyst carrier obtained in Example 1 was impregnated for the second time. The impregnation solution was a mixed solution of lanthanum nitrate and cerium (III) nitrate. The molar ratio of La:Ce was 9:1, and the total concentration of La and Ce was 0.5 mol / L. The impregnated material was dried and calcined at 450°C to obtain La2O3-CeO2 and La2O3-modified Al2O3. Due to the two modifications, the pore volume of the carrier was further reduced to 0.5 cm 3 / g. Figure 4 The XRD pattern shown shows that the modified support has no characteristic peaks of La2O3 and CeO2, and the lattice size of Al2O3 increases to 2.7 nm, indicating that the second modifier can spread well on the surface of the first modified support.
[0043] Example 4 Example of one-step loading of La2O3-CeO2 on catalyst carrier A mixed solution of lanthanum nitrate and cerium (III) nitrate was impregnated on the catalyst carrier Al2O3, the molar ratio of La:Ce was 9:1, and the total concentration of La and Ce was 0.5 mol / L. The impregnated material was dried and calcined at 450°C to obtain La2O3-CeO2 modified Al2O3. Figure 5 The XRD results show that the characteristic peak of CeO2 has not been observed. XRD shows that the lattice size of Al2O3 increases from 2.3 nm to 2.7 nm. BET data show that the pore volume of Al2O3 is significantly reduced to only 0.65 cm 3 / g. The amount of La2O3-CeO2 loaded on the Al2O3 carrier in one step is much less than that obtained by two-step impregnation in Example 3, and the characteristic peaks of CeO2 and La2O3 are not obvious. This shows that La2O3-CeO2 can be fully spread on the carrier surface as in Example 3.
[0044] Example 5 Loading the Second Surface Modifier Cr2O3-TiO2 on the SiO2 Carrier A mixed solution of chromium (III) sulfate and titanyl sulfate was impregnated on the TiO2-modified carrier SiO2 described in Example 2, with a molar ratio of Cr:Ti of 9:1 and a total concentration of Ti and Cr of 0.5 mol / L. After drying, the carrier was calcined at 550°C to obtain Cr2O3-TiO2-modified SiO2. Figure 6The XRD results show that the characteristic peaks of Cr2O3 and TiO2 were not observed. The lattice size of SiO2 increased from 3.4 nm to 3.6 nm. The BET data showed that the pore volume of SiO2 further increased from 0.72 cm 3 / g is reduced to 0.60 cm 3 This example shows that the second modifying agent can be well spread on the surface of the first modified carrier.
[0045] Example 6 Example of loading Cr2O3-TiO2 on a catalyst carrier A mixed solution of chromium (III) sulfate and titanyl sulfate was directly impregnated on the catalyst carrier SiO2, with a molar ratio of Cr:Ti of 9:1 and a total concentration of Ti and Cr of 0.5 mol / L. The impregnated material was dried and calcined at 550°C to obtain Cr2O3-TiO2-modified SiO2. Figure 7 The XRD results show that the characteristic peak of TiO2 is observed, and the corresponding TiO2 lattice size is about 4.4 nm; the XRD does not observe the characteristic peak of Cr2O3. XRD shows that the lattice size of SiO2 increases from 3.4 nm to 3.7 nm; BET data show that the pore volume of SiO2 is significantly reduced, about 0.61 cm 3 Although the amount of Cr2O3-TiO2 loaded on the SiO2 carrier is much less than that obtained by two-step impregnation in Example 3, the characteristic peaks of TiO2 are more obvious. This indicates that the directly loaded Cr2O3-TiO2 fails to spread fully on the carrier surface as in Example 3, and nano-TiO2 particles with a crystalline structure are formed in the micropores of SiO2.
[0046] Example 7 Example of loading Cr2O3-TiO2 on a catalyst carrier Cr2O3-TiO2 modified SiO2 was obtained by the preparation method of Example 5. Then, it was impregnated for the third time with a 0.2 mol / L AgNO3 solution and dried and calcined in the same way to obtain Ag / TiO2-Cr2O3 / Al2O3 catalyst. -1 ) to conduct formaldehyde removal experiments. The formaldehyde concentration used in the experiment was about 100 ppm. The formaldehyde conversion rates obtained by the catalyst at different temperatures are as follows: Figure 8 As shown in Figure 2, at high temperatures of 80°C and 90°C, the conversion rates can reach 90% and 100%, respectively. After that, the conversion rate drops significantly as the temperature decreases, and at 30°C, the conversion rate is only 4.5%.
[0047] Example 8 Example of adjusting the ratio of surface modifier TiO2-Cr2O3 The preparation method in Example 5 was used to control the total concentration of Ti and Cr to 0.5 mol / L, but the ratio of Ti to Cr was changed from 0 to 1 to obtain a series of catalyst supports. The third impregnation was performed on these catalyst supports. The impregnation solution was a 0.2 mol / L AgNO3 solution. The impregnated product was dried and calcined at 550°C to obtain a series of dealdehyde catalysts. At a high gas velocity (GHSV = 47000 hr -1 ) to conduct formaldehyde removal experiments. The formaldehyde concentration used in the experiment was about 100 ppm. The formaldehyde conversion rates obtained by various catalysts at different temperatures are as follows: Fig. 9 As shown. The experimental results show that when Ti:Cr=1:9, the catalyst has a relatively high conversion rate in each temperature range (90, 60 and 25 ℃). Therefore, the actual catalyst can be expressed as Ag / Cr2O3-TiO2 / TiO2 / SiO2. Because the first surface modifier and the second surface modifier both contain TiO2, the above catalyst can be abbreviated as Ag / TiO2-Cr2O3 / SiO2.
[0048] Example 9 Example of adjusting the ratio of surface modifier La-CeO2 The preparation method in Example 4 was used to control the total concentration of La and Ce to 0.5 mol / L, but the ratio of La to Ce was changed from 0 to 1 to obtain a series of catalyst supports. The third impregnation was performed on these catalyst supports. The impregnation solution was a 0.2 mol / L AgNO3 solution. The impregnated product was dried and calcined at 450°C to obtain a series of dealdehyde catalysts. At a high gas velocity (GHSV = 47000 hr -1 ) to conduct formaldehyde removal experiments. The formaldehyde concentration used in the experiment was about 100 ppm. The formaldehyde conversion rates obtained by various catalysts at different temperatures are as follows: Fig.10 As shown. The experimental results show that when La:Ce=1:9, the catalyst has a relatively high conversion rate in each temperature range (90, 60 and 25 ℃). Therefore, the actual catalyst can be expressed as Ag / La2O3-CeO2 / La2O3 / Al2O3. Because both the first surface modifier and the second surface modifier contain La2O3, the above catalyst can be abbreviated as Ag / La-CeO2 / Al2O3.
[0049] Example 10 Example of adjusting the concentration of main catalyst Ag2O The molar ratio of La:Ce in Example 9 was fixed at 9:1, and the concentration of AgNO3 in the impregnation solution was adjusted from 0 to 1 mol / L to obtain a series of dealdehyde catalysts. -1The conversion rate of the catalyst at 25, 60, and 90 °C was tested. According to the experimental results, when the concentration of AgNO3 is 0.5 mol / L, the catalyst Ag loading is about 5%, and the conversion rate is the highest at this time. When the Ag loading is further increased, the conversion rate decreases at 60 and 25 °C. It is proved that excessive Ag may cause the aggregation of catalyst metal silver clusters and affect the activity of the catalyst. When the concentration of AgNO3 impregnation solution is 0.2 mol / L, the conversion rate at 90 °C is increased by 143% compared with the concentration of 0.1 mol / L.
[0050] Example 11 Example of the Effect of Alkali Metal Na and K as Co-catalysts The method of Example 10 was used to prepare the dealdehyde catalyst. The concentration of the AgNO3 impregnation solution was 0.2 mol / L, and the catalyst contained about 2 wt% silver. 0.1 mol / L of sodium nitrate or potassium nitrate was added to the impregnation solution as a precursor of the co-catalyst. -1 , the effects of promoters Na and K were investigated when the formaldehyde concentration was 100 ppm ( Fig.12 As shown). The results show that at 30-50 ℃, the performance of Na and K as co-catalysts is similar; after the temperature rises to 60 ℃, the conversion rate of the catalyst containing K is much higher than that of the catalyst containing Na. The catalyst containing K can achieve a conversion rate of 98% at 85 ℃ and a conversion rate of about 50% at 70 ℃. Therefore, K is a relatively good co-catalyst. The use of co-catalyst K can enable the catalyst with a silver content of 2wt% to achieve complete conversion of formaldehyde, avoiding the use of catalysts with high silver content.
[0051] Example 12 Noble Metal Platinum Catalyst The price of precious metal platinum (Pt) is 50 times that of silver. When the silver content is 2wt%, the equivalent Pt content is 0.04wt%. The Ag in the catalyst Ag / La-CeO2 / Al2O3 was replaced with an equivalent amount of Pt and tested according to the reaction conditions of Example 9. Because the Pt content was too low, the catalyst had only a 13.5% formaldehyde conversion rate at 90°C, which was much lower than the formaldehyde conversion rate of the silver-based catalyst ( Fig.13 as shown).
[0052] Example 13 Copper-based catalyst The Ag in the catalyst Ag / La-CeO2 / Al2O3 was replaced with cheaper Cu with a loading of 6wt%. The test conditions were the same as those in Example 9. Although Cu and Ag are both Group 11 elements, the low-temperature activity of Cu is lower than that of Ag, with only a 40% conversion rate at 90°C ( Fig.14 As shown in Figure 2, the price of Cu is only one thousandth of that of Ag, so a lower GHSV or longer residence time can be used to obtain a conversion rate similar to that of Ag catalyst.
[0053] Example 14 Example of Co3O4 Similar to Example 9 and Example 10, the active component Ag in Ag / La-CeO2 / Al2O3 was replaced with Co as the catalyst active component, and the content of Co was 5wt%. The conversion rate of the catalyst was only 29.5% at 90°C. Since the price of Co is much higher than that of Cu, the Co-based catalyst has no advantages in performance and price.
[0054] Example 15 High, medium and low formaldehyde concentrations At GHSV of 15700 hr -1 , the effect of formaldehyde concentration on the formaldehyde conversion rate of the catalyst was investigated when the catalyst was K-Ag / La-CeO2 / Al2O3. At a low concentration of 1ppm, the formaldehyde conversion rate can always be maintained at around 99%. The formaldehyde in a normal living environment can be reduced to within a safe range of 0.08ppm. The formaldehyde conversion rate at a concentration of 10ppm is also significantly better than that of 70ppm. At 30℃, the formaldehyde conversion rate is 10.8%, and at 70℃, the formaldehyde conversion rate can reach 76.1%. When the formaldehyde concentration is 70ppm, the formaldehyde conversion rate at 70℃ is 50%.
[0055] Example 16 Catalytic Comparative Sample Ag / Al2O3 At GHSV of 15700h -1 The conversion rates of Ag / Al2O3, Ag / CeO2 / Al2O3 and K-Ag / La-CeO2 / Al2O3 catalysts at different temperatures were tested under the conditions. According to the experimental results, the conversion rate of Ag / Al2O3 catalyst was 0 at 50°C, while Ag / CeO2 / Al2O3 and K-Ag / La-CeO2 / Al2O3 still had 8.7% and 15.8% conversion rates respectively. At 90°C, the conversion rate of Ag / Al2O3 catalyst was only 35.9%, while the conversion rates of Ag / CeO2 / Al2O3 and K-Ag / La-CeO2 / Al2O3 were 93.8% and 100% respectively. The conversion rate of K-Ag / La-CeO2 / Al2O3 was increased by 178% compared with Ag / Al2O3.
[0056] Example 17 Adsorption of formaldehyde At room temperature 25 ℃, GHSV = 15700h -1 The adsorption performance of K-Ag / La-CeO2 / Al2O3 catalyst was tested in air atmosphere and nitrogen atmosphere. Fig.18It can be seen that the formaldehyde adsorption removal rate changes with time. In the early stage, the formaldehyde adsorption removal rate is close to 0, and after a period of time, the formaldehyde removal rate gradually decreases. When the formaldehyde adsorption removal rate drops to 50%, it only takes 171 minutes in nitrogen atmosphere, while it takes 255 minutes in air atmosphere. According to this time, each gram of catalyst can adsorb about 2.6×10 -4 mol formaldehyde, and each gram of catalyst can adsorb about 4.0×10 -4 mol formaldehyde.
Claims
1. A method for preparing a low-temperature catalytic oxidation catalyst, characterized in that: A three-step impregnation method is adopted to respectively impregnate the first surface modifier, the second surface modifier and the catalyst active component on the catalyst carrier.
2. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The catalyst carrier is one of aluminum oxide, silicon oxide, SiO2-Al2O3, molecular sieve or calcined hydrotalcite.
3. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The first surface modifier is a transition metal oxide that can spread on the surface of the catalyst support.
4. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The first surface modifier is a transition metal oxide having the same valence state as the metal in the catalyst carrier but a different metal element.
5. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The second surface modifier is a transition metal oxide rich in oxygen vacancies and covers the surface of the first surface modifier in the form of a thin film.
6. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The second surface modifier is at least one of the metal oxides CuO, ZnO, CeO2, ZrO2, TiO2, WO3 or MoO3, or a low-valent doped metal oxide is simultaneously introduced into the metal oxide, wherein the low-valent state means that the valence of the doped metal is lower than the one or two valences of the doped metal.
7. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The second surface modifier contains at least one component that is the same as the oxide in the first surface modifier; When the second surface modifier can spread on the surface of the catalyst support, only the second surface modifier needs to be used, and the first impregnation and the first surface modifier are omitted.
8. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: The catalyst active components include main catalysts Ag2O, Cu2O, FeO, Co3O4, NiO, MnO x At least one of the above and at least one of the corresponding oxides of the co-catalysts Li, Na, K, Cs.
9. The method for preparing a low-temperature catalytic oxidation catalyst according to claim 1, characterized in that: In the impregnation of the first and second surface modifiers, the precursor of the metal oxide is the nitrate, sulfate, chloride, acetate or oxalate corresponding to the metal oxide; the catalyst carrier with the surface modifier is first obtained by drying and calcining, and the surface-modified carrier is obtained after secondary impregnation-drying-calcination, and then the surface-modified carrier is impregnated with the active component for the third time, and the solution used is the nitrate, sulfate, acetate, oxalate or chloride solution of the metal corresponding to the active component except silver, and the low-temperature catalytic oxidation catalyst is obtained after drying and calcining again; in the obtained low-temperature catalytic oxidation catalyst, the carrier mass accounts for 80-90wt%, the total proportion of the first and second surface modifiers is 7-19wt%, and the active component is 1-3wt%.
10. Use of the low-temperature catalytic oxidation catalyst obtained by the preparation method according to any one of claims 1 to 9 in a dealdehyde reaction.
Citation Information
Patent Citations
Normal-temperature high-effective formaldehyde catalytic-oxidizing catalyst, preparation method, and application thereof
CN107096527A
Compound carrier catalyst for room temperature catalysis of formaldehyde and preparation method thereof
CN107398272A
Noble metal-loaded type catalyst and preparation method and application thereof
CN108176399A
High temperature stable catalyst and process for preparing same
US4738946A