Ce-Mn bimetallic oxide catalyst as well as preparation method and application thereof

Through the combined use of Ce-Mn bimetal oxide catalyst and ozone, the efficient degradation and biochemical improvement of phenolic organic matter in coal gasification wastewater is solved, and efficient and stable wastewater treatment is achieved, which is suitable for industrial applications.

CN118988291APending Publication Date: 2024-11-22YILI NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410310641.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high concentration and stable structure of phenolic organic matter in coal gasification wastewater limit the effect of wastewater biochemical treatment. Traditional treatment methods are difficult to meet the emission requirements, and biochemical methods have high requirements for wastewater biochemical properties, so it is difficult for the existing technology to achieve efficient degradation.

Method used

Ce-Mn bimetal oxide catalyst is prepared by hydrothermal method, combined with ozone catalyst, and phenolic organic matter in coal gasification wastewater is degraded to improve its biochemical properties. The specific steps include hydrothermal reaction of Ce(NO3)3 and Mn(NO3)2 with the support in sodium hydroxide to form Ce-Mn bimetallic hydroxide, and then calcining to obtain the Ce-Mn bimetallic oxide catalyst. And treat phenolic wastewater with ozone in the reactor.

Benefits of technology

It achieves efficient degradation of phenolic organic matter, improves the biochemical properties of wastewater, has high degradation rate and strong stability, is suitable for industrial wastewater treatment, has low cost and has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005092251500000031
    Figure GDA0005092251500000031
  • Figure GDA0005092251500000051
    Figure GDA0005092251500000051
Patent Text Reader

Abstract

The invention discloses a Ce-Mn bimetallic oxide catalyst and a preparation method and application thereof, and belongs to the technical field of catalysts.The preparation method comprises the steps that firstly, a catalyst carrier is added into deionized water to be stirred to form turbid liquid; adding Ce (NO3) 3 and Mn (NO3) 2 into the turbid liquid obtained in the step 1, stirring, dissolving and standing to obtain a double-metal hydroxide precursor solution; adding sodium hydroxide into the bimetallic hydroxide precursor solution in the step 2 for hydrothermal reaction, washing and drying solids obtained by reaction separation to obtain Ce-Mn bimetallic hydroxide loaded on a carrier, and finally grinding the Ce-Mn bimetallic hydroxide and calcining at 600 DEG C to obtain the Ce-Mn bimetallic oxide catalyst loaded on the carrier. The method is used for degrading phenolic organic matters in coal gasification wastewater by an ozone catalyst. The preparation method is simple and efficient, and the method for degrading the phenolic organic matters in the coal gasification wastewater through ozone catalytic oxidation by taking the Ce-Mn bimetallic oxide as the catalyst has the characteristics of high degradation rate, high stability and high feasibility, and has a wide application prospect in industrial wastewater treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a Ce-Mn bimetallic catalyst for degrading phenolic organic matter in coal gasification wastewater, and a preparation method and application thereof. Background Art

[0002] Coal gasification wastewater contains a variety of toxic and hazardous substances, among which phenolic compounds are typical high-concentration, highly toxic organic pollutants in coal gasification wastewater. They usually exist in the form of monophenols such as phenol, methylphenol, and alkylphenol, and also contain a variety of polyphenols, such as resorcinol and hydroquinone. However, most phenolic substances have great limitations on the treatment effect of wastewater biochemical treatment units due to their biological toxicity and stable structure. The discharge of untreated phenolic wastewater will cause serious health problems to the public and aquatic ecosystems. The current traditional treatment methods are not enough to meet the discharge requirements of wastewater treatment. Therefore, the development of efficient and environmentally friendly methods for the treatment and degradation of phenolic substances has become a current research hotspot.

[0003] The composition of coal gasification wastewater is complex, and a single treatment process is difficult to achieve complete degradation of high-concentration complex organic pollutants. According to a comprehensive analysis of the treatment technologies currently used in the coal gasification industry at home and abroad, it can be divided into three categories: physical methods, chemical methods and biochemical methods. Although physical and chemical methods are simple, efficient and effective in treating wastewater, they will cause high cost investment for enterprises and are not suitable for industrial applications. The biochemical treatment method uses the metabolism of microorganisms to achieve the degradation of pollutants in wastewater and achieve the purpose of water purification. The biochemical method has high requirements for the biodegradability of wastewater. Coal gasification wastewater contains a large amount of phenolic substances with poor biodegradability. Therefore, improving the biodegradability of coal gasification wastewater has become a problem to be solved. Although a variety of process technologies are widely used in the treatment of phenolic organic matter in coal gasification wastewater, they have their own advantages and disadvantages in actual application and operation. Therefore, seeking efficient and feasible enhanced technologies to achieve efficient degradation of phenolic pollutants and improve biodegradability has become a necessary condition to ensure the stable operation of coal gasification wastewater biochemical treatment units. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a Ce-Mn bimetallic oxide catalyst, which can degrade phenolic organic matter in coal gasification wastewater and improve its biodegradability.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a Ce-Mn bimetallic oxide catalyst comprises the following steps:

[0007] Step 1: Add the catalyst support into deionized water and stir to form a suspension;

[0008] Step 2: Add Ce(NO3)3 and Mn(NO3)2 to the suspension of step 1, stir and dissolve, and let stand to obtain a double metal hydroxide precursor solution;

[0009] Step three: adding sodium hydroxide to the double metal hydroxide precursor solution in step two for hydrothermal reaction; washing and drying the solid separated by the reaction to obtain a Ce-Mn double metal hydroxide supported on a carrier; finally, grinding the Ce-Mn double metal hydroxide and calcining at 600° C. to obtain a Ce-Mn double metal oxide catalyst supported on a carrier.

[0010] The MnO2 and CeO2 theoretically generated from Ce(NO3)3 and Mn(NO3)2 in step 2 account for 2.5-12.5% ​​of the carrier mass in step 1, respectively.

[0011] Preferably, the MnO2 and CeO2 theoretically generated from Ce(NO3)3 and Mn(NO3)2 in step 2 account for 10% of the mass of the carrier in step 1 respectively.

[0012] The Ce-Mn bimetallic oxide catalyst is used for the ozone catalyst degradation of phenolic organic matter in coal gasification wastewater, specifically: the Ce-Mn3 bimetallic composite catalyst and ozone are passed through the coal gasification phenol-containing wastewater to degrade the phenolic substances into acetic acid, oxalic acid, hydroquinone, benzoquinone, catechol and other small molecular organic compounds, and finally degraded to generate CO2 and H2O, thereby improving its biodegradability.

[0013] When the COD (chemical oxygen demand) of phenolic organic matter in the coal gasification wastewater is greater than 300 mg / L and the total phenol concentration is greater than 400 mg / L, the bimetallic composite catalyst and ozone introduced into the ozone catalytic reactor are 3-5 g / L and 2-4 L / min, respectively; when the COD (chemical oxygen demand) of phenolic organic matter in the coal gasification wastewater is less than 300 mg / L and the total phenol concentration is less than 400 mg / L, the bimetallic composite catalyst and ozone introduced into the ozone catalytic reactor are 1-3 g / L and 0.5-2 L / min, respectively;

[0014] The catalyst carrier in step one includes but is not limited to γ-Al2O3, activated carbon, molecular sieve, gasifier ash and other porous, highly dispersible, highly adsorbent and highly stable catalyst carriers. The γ-Al2O3 is in a white fluffy powder state with an average particle size of 20nm. Its surface is rich in hydroxyl groups (-OH), which can effectively promote the formation of hydroxyl radicals.

[0015] In step 2, stir to dissolve and then let stand for 12 hours.

[0016] Furthermore, the treatment in step three includes the following steps: adding excess sodium hydroxide solution to the precursor solution that has been allowed to stand in step two and stirring for 30 minutes, then transferring it to a polytetrafluoroethylene hydrothermal kettle and hydrothermally reacting it at 120°C for 4 hours; after that, when the hydrothermal kettle is cooled to room temperature, centrifuging the mixture to obtain a viscous solid, then washing it with deionized water until the pH of the rinse water is neutral, then washing it with anhydrous ethanol and centrifuging it, and drying it at 85°C for 12 hours; finally, grinding the solid in an agate mortar to form a powder state, and calcining it at 600°C in a muffle furnace for 2 hours.

[0017] The Ce-Mn bimetallic oxide catalyst in step three can be used for targeted ozone catalytic oxidation and degradation of phenolic organic matter in coal gasification wastewater.

[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention first prepares the Ce-Mn double metal hydroxide loaded on the carrier by a hydrothermal method in one step, and then obtains the corresponding oxide catalyst Ce-Mn by calcination, which is simple and efficient; (2) The MnO2 in the double metal oxide has the advantages of high redox potential, environmental protection and low cost, and the electron-rich Mn 2+ The presence of catalytic active sites such as surface oxygen vacancies will promote the decomposition of ozone to produce reactive oxygen species (ROS). The addition of Ce element can produce more surface vacancies and improve the activity of the catalyst. Ce and Mn work synergistically to achieve efficient degradation of phenolic organic matter in coal gasification wastewater and improve its biodegradability. (3) The method of using Ce-Mn bimetallic oxide as catalyst for ozone catalytic oxidation degradation of phenolic organic matter in coal gasification wastewater has the characteristics of high degradation rate, strong stability and high feasibility, and has broad application prospects in industrial wastewater treatment. DETAILED DESCRIPTION

[0019] In order to make the technical means, creative features, objectives and effects of the present invention easier to understand, the present invention is further described below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0020] Embodiment 1:

[0021] A method for preparing a Ce-Mn bimetallic catalyst comprises the following steps:

[0022] Step 1: Select γ-Al2O3 with high porosity, high dispersibility, strong adsorption and strong stability as the carrier. Weigh 10g of γ-Al2O3, add 34.5mL of deionized water and stir to form a suspension;

[0023] Step 2: Add 2.5231 g Ce(NO3)3·6H2O and 4.1138 g 50 wt% Mn(NO3)2 aqueous solution to the suspension in step 1, stir and dissolve, and let stand to obtain a precursor solution;

[0024] Step 3: Add 8 mol / L sodium hydroxide solution to the precursor solution in step 2, stir for 30 minutes, then transfer it to a polytetrafluoroethylene hydrothermal reactor, and perform hydrothermal reaction at 120°C for 4 hours. After the hydrothermal reactor cools to room temperature, centrifuge the mixture to obtain a viscous solid, then wash it with deionized water until the pH of the rinse water is neutral, then wash it with anhydrous ethanol and centrifuge it, dry it at 85°C for 12 hours, and finally grind the dried solid into a powder state and calcine it at 600°C in a muffle furnace for 2 hours to finally obtain a Ce-Mn / γ-Al2O3 bimetallic composite catalyst.

[0025] Embodiment 2:

[0026] Except that the carrier in step 1 is gasification furnace ash CGA, the other steps of this embodiment are the same as those of embodiment 1, and the Ce-Mn / CGA bimetallic composite catalyst is finally obtained.

[0027] 1g of Ce-Mn / γ-Al2O3 or Ce-Mn / CGA bimetallic composite catalyst prepared in Examples 1 and 2 was respectively loaded into an ozone catalytic reactor with phenol, p-cresol, o-cresol, simulated phenol-containing wastewater (composed of phenol, p-cresol, o-cresol) or coal gasification phenol-containing wastewater with a COD of 200mg / L, and then ozone was introduced into the reactor at a rate of 2L / min. The removal rate (%) was calculated and summarized as shown in Table 1.

[0028] Table 1

[0029]

[0030] The ozone catalytic reactor consists of an oxygen cylinder, an ozone generator, a gas flowmeter, a reactor and a tail gas absorption device. At the beginning of the reaction, the oxygen cylinder is opened, and the ozone generator is pre-blown for 5 minutes. When the gas flow is stable and the outlet pressure is controlled at 0.1Mpa, 1g of the prepared catalyst is added, and an equal volume of coal gasification phenol-containing wastewater (or phenol, p-cresol, o-cresol, simulated phenol-containing wastewater) is added to the reactor. Then the ozone generator is turned on, and oxygen is discharged through the high-voltage discharge inside the ozone generator to generate ozone. By adjusting the gas flow of the ozone generator, the output of ozone is controlled to be 2L / min. A sampling port is reserved on the side wall of the reactor. Samples are taken regularly during the experiment to measure various indicators. The waste gas generated in the experiment is discharged after being absorbed by a 20% concentration KI solution.

[0031] Comparative Example 1:

[0032] A method for preparing a Ce catalyst comprises the following steps:

[0033] Step 1: Select γ-Al2O3 with high porosity, high dispersibility, strong adsorption and strong stability as the carrier. Weigh 10g of γ-Al2O3, add 34.5mL of deionized water and stir to form a suspension;

[0034] Step 2: Add 1.2615g, 2.5231g, 3.7846g, 5.0461g and 6.3055g of Ce(NO3)3·6H2O to the suspension of step 1, stir and dissolve to obtain a precursor solution; the percentage of CeO2 in 1.2615g, 2.5231g, 3.7846g, 5.0461g and 6.3055g of Ce(NO3)3·6H2O is 5%, 10%, 15%, 20% and 25% of the carrier mass respectively.

[0035] Step 3: Add 8 mol / L sodium hydroxide solution to the precursor solution in step 2, stir for 30 minutes, then transfer it to a polytetrafluoroethylene hydrothermal reactor, and perform hydrothermal reaction at 120°C for 4 hours. After the hydrothermal reactor cools to room temperature, centrifuge the mixture to obtain a viscous solid, then wash it with deionized water until the pH of the rinse water is neutral, then wash it with anhydrous ethanol and centrifuge it, dry it at 85°C for 12 hours, and finally grind the dried solid into a powder state and calcine it at 600°C in a muffle furnace for 2 hours to finally obtain a CeO2 / γ-Al2O3 catalyst.

[0036] Comparative Example 2:

[0037] A method for preparing a Mn catalyst comprises the following steps:

[0038] Step 1: Select γ-Al2O3 with high porosity, high dispersibility, strong adsorption and strong stability as the carrier. Weigh 10g of γ-Al2O3, add 34.5mL of deionized water and stir to form a suspension;

[0039] Step 2: Add 2.0568g, 4.1138g, 6.1706g, 8.2274g, 12.6149g of 50wt% Mn(NO3)2 aqueous solution to the suspension of step 1, stir and dissolve, and let stand to obtain a precursor solution; 2.0568g, 4.1138g, 6.1706g, 8.2274g, 12.6149g of 50wt% Mn(NO3)2 aqueous solution, the percentage of MnO2 in the carrier mass is 5%, 10%, 15%, 20%, 25% respectively;

[0040] Step 3: Add 8 mol / L sodium hydroxide solution to the precursor solution in step 2, stir for 30 minutes, then transfer it to a polytetrafluoroethylene hydrothermal reactor, and perform hydrothermal reaction at 120°C for 4 hours. After the hydrothermal reactor cools to room temperature, centrifuge the mixture to obtain a viscous solid, then wash it with deionized water until the pH of the rinse water is neutral, then wash it with anhydrous ethanol and centrifuge it, dry it at 85°C for 12 hours, and finally grind the dried solid into a powder state and calcine it at 600°C in a muffle furnace for 2 hours to finally obtain a MnO2 / γ-Al2O3 catalyst.

[0041] The catalysts and phenol solutions prepared in Comparative Examples 1 and 2 were loaded into an ozone catalytic reactor, and then ozone was introduced therein, and the removal rate (%) was calculated and summarized to determine the optimal ratio conditions. After that, the simulated phenol-containing wastewater was used as the research object, and the reaction test was performed. The results are shown in Table 2. When the final oxide state (CeO2, MnO2) accounted for 10% of the carrier, the removal rates of phenol by the obtained Ce / γ-Al2O3 metal catalyst, MnO2 / γ-Al2O3 metal catalyst, and Ce-Mn / γ-Al2O3 bimetallic composite catalyst were 67.62%, 83.94%, and 94.32%, respectively. It can be seen that the effect of the two loads is better than that of a single one.

[0042] Table 2

[0043]

[0044] The above description is only an example for clearly explaining the present application, and is not intended to limit the implementation methods of the present application. Any obvious changes or modifications derived from the technical solution of the present application are still within the scope of protection of the present application. Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, it should be understood by those skilled in the art that various changes can be made to it in form and detail without departing from the scope defined by the claims of the present invention.

Claims

1. A method for preparing a Ce-Mn bimetallic oxide catalyst, It is characterized in that The following steps are involved: Step 1: Add the catalyst support into deionized water and stir to form a suspension; Step 2: Ce(NO 3 ) 3 and Mn(NO 3 ) 2 Add to the suspension in step 1, stir and dissolve, and let stand to obtain a double metal hydroxide precursor solution; Step 3: adding sodium hydroxide to the double metal hydroxide precursor solution in step 2 for hydrothermal reaction, washing and drying the solid separated by the reaction to obtain Ce-Mn double metal hydroxide supported on the carrier, and finally grinding the Ce-Mn double metal hydroxide and calcining at 600° C. to obtain a Ce-Mn double metal oxide catalyst supported on the carrier. In the step 2, Ce(NO 3 ) 3 and Mn(NO 3 ) 2 Theoretical generation of MnO 2 and CeO 2 They account for 2.5-12.5% ​​of the mass of the carrier in step one respectively.

2. The method for preparing the Ce-Mn bimetallic oxide catalyst according to claim 1, It is characterized in that In the step 2, Ce(NO 3 ) 3 and Mn(NO 3 ) 2 Theoretical generation of MnO 2 and CeO 2 Each accounts for 10% of the mass of the carrier in step 1.

3. The method for preparing the Ce-Mn bimetallic oxide catalyst according to claim 1, It is characterized in that The catalyst carrier in step 1 includes γ-Al 2 O 3 , activated carbon, molecular sieve, gasifier ash.

4. The method for preparing the Ce-Mn bimetallic oxide catalyst according to claim 1, It is characterized in that The treatment in step three includes the following steps: adding excess sodium hydroxide solution to the precursor solution that has been allowed to stand in step two and stirring for 30 minutes, then transferring it to a polytetrafluoroethylene hydrothermal kettle and hydrothermally reacting it at 120°C for 4 hours; after that, when the hydrothermal kettle is cooled to room temperature, centrifuging the mixture to obtain a viscous solid, then washing it with deionized water until the pH of the rinse water is neutral, then washing it with anhydrous ethanol and centrifuging it, and drying it at 85°C for 12 hours; finally, grinding the solid in an agate mortar to form a powder state, and calcining it at 600°C in a muffle furnace for 2 hours.

5. The Ce-Mn bimetallic oxide catalyst prepared by the preparation method according to any one of claims 1 to 4.

6. The Ce-Mn bimetallic oxide catalyst according to claim 5 is used as an ozone catalyst to degrade phenolic organic matter in coal gasification wastewater.

7. The Ce-Mn bimetallic oxide catalyst according to claim 6 is used as an ozone catalyst to degrade phenolic organic matter in coal gasification wastewater. It is characterized in that Ce-Mn 3 The bimetallic composite catalyst and ozone are passed through coal gasification wastewater containing phenols. When the COD of phenolic organic matter in the coal gasification wastewater is greater than 300 mg / L and the total phenol concentration is greater than 400 mg / L, the bimetallic composite catalyst and ozone introduced into the ozone catalytic reactor are 3-5 g / L and 2-4 L / min, respectively; when the COD of phenolic organic matter in the coal gasification wastewater is less than 300 mg / L and the total phenol concentration is less than 400 mg / L, the bimetallic composite catalyst and ozone introduced into the ozone catalytic reactor are 1-3 g / L and 0.5-2 L / min, respectively.

Citation Information

Patent Citations

  • Method for preparing double-component metallic oxide catalytic ozonation catalyst

    CN102941084A

  • CeOx-MnOx / graphene low-temperature SCR flue gas denitration catalyst and preparation method thereof

    CN104759277A

  • Method for preparing Mn-Ce / Al2O3 catalyst and catalyzing ozonized organic wastewater difficult to degrade

    CN106268783A

  • Preparation method and application of efficient ozone oxidation catalyst

    CN116020486A