Silver-palladium quantum dot anchoring defect titanium dioxide nano array composite photocatalyst as well as preparation method and application thereof
By preparing silver-palladium quantum dot anchoring defective titanium dioxide nanoarray composite photocatalyst, the problem of inability to remove organic pollutants and microorganisms at the same time in the prior art is solved, and efficient degradation and disinfection effect of organic pollutants and microorganisms is achieved.
Patent Information
- Application Number
- CN202411283850.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The lack of bifunctional photocatalysts that can simultaneously remove organic pollutants and microorganisms in the prior art limits the application of titanium dioxide nanomaterials in wastewater treatment.
By preparing silver-palladium quantum dot anchoring defective titanium dioxide nanoarray composite photocatalyst, secondary anodization and cathode reduction methods were used, and combined with chemical reduction methods, a photocatalyst with dual efficacy was prepared.
It significantly improves the degradation efficiency of tetracycline hydrochloride and ciprofloxacin, and can completely inactivate E. coli and significantly disinfect Staphylococcus white within a certain period of time, which is better than traditional titanium dioxide nanomaterials.
Smart Images

Figure CN118988299A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photocatalysis technology, and in particular to a silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst and a preparation method and application thereof. Background Art
[0002] The rapid development of industrialization, urbanization and economic globalization has disrupted the ecological balance, exacerbated the pollution of the ecological environment, and seriously threatened the living environment and health of human beings. Among them, the problems of antibiotic resistance and the spread of pathogenic microorganisms are the most prominent. Therefore, people are more and more in need of multifunctional materials that can continuously degrade antibiotics and inhibit the spread of pathogenic microorganisms.
[0003] Titanium dioxide nanomaterials have attracted much attention due to their green, environmentally friendly and low-cost advantages. However, due to their wide band gap, they only respond to ultraviolet light, which greatly limits their application in the field of photocatalysis. Many scholars have improved the performance of titanium dioxide nanomaterials by adopting strategies such as morphology regulation of titanium dioxide nanomaterials, construction of heterostructures, semiconductor composites, and surface modification of precious metals, but they mainly focus on the removal of organic pollutants. However, actual wastewater treatment requires consideration of both organic pollutants and microorganisms. At present, there is no research on bifunctional photocatalysts that can simultaneously remove organic pollutants and microorganisms. Therefore, the study of bifunctional photocatalysts that can simultaneously remove organic pollutants and microorganisms has good prospects. Summary of the invention
[0004] The purpose of the present invention is to provide a silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst and a preparation method and application thereof in view of the deficiencies in the prior art.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst, comprising the following steps:
[0007] 1) Anodizing the titanium sheet cathode and the titanium mesh anode in a fluorinated ethylene glycol solution to obtain an amorphous titanium dioxide nanoarray;
[0008] 2) annealing the amorphous titanium dioxide nanoarray to obtain anatase titanium dioxide nanoarray;
[0009] 3) using the titanium sheet as an anode and the anatase titanium dioxide nanoarray as a cathode, and performing cathode reduction in a formic acid solution to obtain a defective titanium dioxide nanoarray;
[0010] 4) Under an argon atmosphere, the defective titanium dioxide nanoarray is placed in a Pd-Ag mixed solution, and a sodium borohydride solution is added dropwise to the Pd-Ag mixed solution for reaction, thereby obtaining a silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst.
[0011] Preferably, the anodization temperature in step 1) is 8-12° C., and the distance between the anodized plates is 1-2 cm; the anodization is carried out twice, the voltage of the first anodization is 45-55 V, and the time is 2.5-4.5 h; the voltage of the second anodization is 5-15 V, and the time is 3-10 min.
[0012] Preferably, the fluorinated ethylene glycol solution in step 1) comprises ammonium fluoride, ethylene glycol and water; the mass fraction of ammonium fluoride in the fluorinated ethylene glycol solution is 0.2-0.3%, and the mass fraction of water is 1-3%.
[0013] Preferably, the annealing temperature in step 2) is 400-500° C., the annealing time is 1-3 h, and the annealing heating rate is 1-3° C. / min.
[0014] Preferably, the temperature of the cathode reduction in step 3) is 8-12°C, the plate spacing of the cathode reduction is 1-2 cm, and the current density of the cathode reduction is 4-6 mA / cm 2 The cathode reduction time is 3 to 10 minutes, and the volume fraction of formic acid in the formic acid solution is 5 to 10%.
[0015] Preferably, the Pd-Ag mixed solution in step 4) comprises palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water, and the molar volume ratio of palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water is 0.5-2 mmol:1 mmol:0.025-0.03 mmol:0.75-2.1 mmol:50 mL.
[0016] Preferably, in step 4), the concentration of the sodium borohydride solution is 0.05-0.2 mol / L, the rate of addition is 0.5-2 mL / min, the molar ratio of sodium borohydride in the sodium borohydride solution to silver nitrate in the Pd-Ag mixed solution is 8-10:1; the reaction is carried out under stirring conditions, the stirring speed is 500-700 rpm, and the stirring time is 0.5-2 h.
[0017] The present invention also provides a silver-palladium quantum dot anchored defective titanium dioxide nano-array composite photocatalyst prepared by the preparation method.
[0018] The present invention also provides the use of the silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst in degrading organic pollutants and disinfecting microorganisms.
[0019] Beneficial effects of the present invention:
[0020] The present invention prepares defective titanium dioxide nanoarrays by a method of secondary anodic oxidation+cathode reduction, adopts a chemical reduction method to prepare a silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst, and rationally controls the process parameters in the processes of anodic oxidation, cathode reduction and chemical reduction, so that the silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst has the dual functions of degrading organic pollutants and disinfecting microorganisms; the degradation efficiency of the silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst for tetracycline hydrochloride is 5.38 times higher than that of titanium dioxide at 100 minutes, and the degradation efficiency of the silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst for ciprofloxacin is 5.78 times higher than that of titanium dioxide; and the silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst can completely inactivate Escherichia coli at 200 minutes, and the light disinfecting rate of Staphylococcus aureus is not less than 50%, which is significantly higher than that of titanium dioxide at the same disinfecting time. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The AgPd prepared in Example 1 1.25 / TiO 2 -4.5 Scanning electron microscope image of composite photocatalyst;
[0022] Figure 2 AgPd prepared in Example 2 1.5 / TiO 2 -2.5 Scanning electron microscope image of the composite photocatalyst;
[0023] Figure 3 The AgPd / TiO prepared in Example 3 2 -3.5 Scanning electron microscope image of composite photocatalyst;
[0024] Figure 4 The AgPd / TiO prepared in Example 3 2 -3.5 Photodegradation rate of tetracycline hydrochloride by composite photocatalyst;
[0025] Figure 5 TiO 2 Photodegradation rate of tetracycline hydrochloride by catalyst;
[0026] Figure 6 The AgPd / TiO prepared in Example 3 2 -3.5 Photodegradation rate of ciprofloxacin by composite photocatalyst;
[0027] Figure 7 TiO 2 Photodegradation rate of ciprofloxacin by catalyst;
[0028] Figure 8 The AgPd / TiO prepared in Example 32 -3.5 Photokilling rate of Escherichia coli by composite photocatalyst;
[0029] Fig. 9 TiO 2 Photokilling rate of E. coli by the catalyst;
[0030] Fig.10 The AgPd / TiO prepared in Example 3 2 -3.5 Photokilling rate of composite photocatalyst on Staphylococcus aureus;
[0031] Fig.11 TiO 2 Photokilling rate of catalyst against Staphylococcus aureus. DETAILED DESCRIPTION
[0032] The present invention provides a method for preparing a silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst, comprising the following steps:
[0033] 1) Anodizing the titanium sheet cathode and the titanium mesh anode in a fluorinated ethylene glycol solution to obtain an amorphous titanium dioxide nanoarray;
[0034] 2) annealing the amorphous titanium dioxide nanoarray to obtain anatase titanium dioxide nanoarray;
[0035] 3) using the titanium sheet as an anode and the anatase titanium dioxide nanoarray as a cathode, and performing cathode reduction in a formic acid solution to obtain a defective titanium dioxide nanoarray;
[0036] 4) Under an argon atmosphere, the defective titanium dioxide nanoarray is placed in a Pd-Ag mixed solution, and a sodium borohydride solution is added dropwise to the Pd-Ag mixed solution for reaction, thereby obtaining a silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst.
[0037] In the present invention, the titanium sheet cathode and the titanium mesh anode in step 1) are preferably pretreated, and the pretreatment preferably includes ultrasonic cleaning and drying performed in sequence; the ultrasonic cleaning preferably includes water ultrasonic cleaning, hydrochloric acid ultrasonic cleaning, acetone ultrasonic cleaning and anhydrous ethanol ultrasonic cleaning performed in sequence, and the frequencies of water ultrasonic cleaning, hydrochloric acid ultrasonic cleaning, acetone ultrasonic cleaning and anhydrous ethanol ultrasonic cleaning are independently preferably 30-50kHz, and more preferably 40kHz; the time of ultrasonic cleaning is independently preferably 10 to 20min, and more preferably 15min; the drying temperature is preferably 50 to 80°C, and more preferably 60 to 70°C; the drying time is preferably 20 to 40min, and more preferably 30min.
[0038] In the present invention, the temperature of the anodization in step 1) is preferably 8-12°C, more preferably 9-11°C, and more preferably 10°C; the distance between the anodized plates is preferably 1-2cm, and more preferably 1.5cm; the anodization is preferably carried out twice, and the voltage of the first anodization is preferably 45-55V, more preferably 48-52V, and more preferably 50V; the time is preferably 2.5-4.5h, more preferably 3.3-3.8h, and more preferably 3.5h; the voltage of the second anodization is preferably 5-15V, more preferably 8-13V, and more preferably 10V; the time is preferably 3-10min, more preferably 5-8min, and more preferably 6min.
[0039] In the present invention, the fluorinated ethylene glycol solution in step 1) preferably comprises ammonium fluoride, ethylene glycol and water; the mass fraction of ammonium fluoride in the fluorinated ethylene glycol solution is preferably 0.2-0.3%, more preferably 0.22-0.28%, more preferably 0.25%; the mass fraction of water is preferably 1-3%, more preferably 1.5-2.5%, more preferably 2%.
[0040] In the present invention, after the anodization in step 1) is completed, the amorphous titanium dioxide nanoarray is preferably cleaned and dried, and the cleaning preferably includes deionized water cleaning and anhydrous ethanol cleaning in sequence, and the number of cleanings is independently preferably 2 to 4 times, and more preferably 3 times; the drying temperature is preferably 50 to 80°C, and more preferably 60 to 70°C; the drying time is preferably 20 to 40 minutes, and more preferably 30 minutes.
[0041] In the present invention, the annealing temperature in step 2) is preferably 400-500°C, more preferably 430-480°C, and more preferably 450°C; the annealing time is preferably 1-3h, more preferably 1.5-2.5h, and more preferably 2h; the annealing heating rate is preferably 1-3°C / min, more preferably 1.5-2.5°C / min, and more preferably 2°C / min.
[0042] In the present invention, the titanium sheet in step 3) is preferably pretreated, and the pretreatment preferably includes ultrasonic cleaning and drying performed in sequence; the ultrasonic cleaning preferably includes water ultrasonic cleaning, hydrochloric acid ultrasonic cleaning, acetone ultrasonic cleaning and anhydrous ethanol ultrasonic cleaning performed in sequence, and the frequencies of water ultrasonic cleaning, hydrochloric acid ultrasonic cleaning, acetone ultrasonic cleaning and anhydrous ethanol ultrasonic cleaning are independently preferably 30-50kHz, and more preferably 40kHz; the time of ultrasonic cleaning is independently preferably 10 to 20min, and more preferably 15min; the drying temperature is preferably 50 to 80°C, and more preferably 60 to 70°C; the drying time is preferably 20 to 40min, and more preferably 30min.
[0043] In the present invention, the temperature of the cathode reduction in step 3) is preferably 8-12°C, more preferably 9-11°C, and more preferably 10°C; the plate spacing of the cathode reduction is preferably 1-2 cm, more preferably 1.5 cm; the current density of the cathode reduction is preferably 4-6 mA / cm 2 , more preferably 4.5 to 5.5 mA / cm 2 , more preferably 5 mA / cm 2 The cathode reduction time is preferably 3 to 10 min, more preferably 4 to 8 min, and more preferably 5 to 6 min; the volume fraction of formic acid in the formic acid solution is preferably 5 to 10%, more preferably 6 to 9%, and more preferably 7 to 8%.
[0044] In the present invention, after the cathode reduction in step 3) is completed, the defective titanium dioxide nanoarray is preferably cleaned and dried, and the cleaning preferably includes deionized water cleaning and anhydrous ethanol cleaning in sequence, and the number of cleanings is independently preferably 2 to 4 times, and more preferably 3 times; the drying temperature is preferably 50 to 80°C, and more preferably 60 to 70°C; the drying time is preferably 50 to 80 minutes, and more preferably 60 to 70 minutes.
[0045] In the present invention, the defective titanium dioxide nanoarray in step 3) is preferably a defective titanium dioxide nanoarray rich in oxygen vacancies.
[0046] In the present invention, the Pd-Ag mixed solution in step 4) is preferably aerated in argon before adding the defective titanium dioxide nanoarray, and the flow rate of argon is preferably 3-8 mL / min, more preferably 5 mL / min; aeration is preferably carried out during stirring, and the stirring speed is preferably 500-700 rpm, more preferably 600 rpm; the stirring time is preferably 10-30 min, more preferably 20 min.
[0047] In the present invention, before the sodium borohydride solution is added dropwise in step 4), the Pd-Ag mixed solution is preferably stirred, and the stirring speed is preferably 500-700 rpm, more preferably 600 rpm; the stirring time is preferably 20-40 min, more preferably 30 min.
[0048] In the present invention, the Pd-Ag mixed solution in step 4) preferably comprises palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water, and the molar volume ratio of palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water is preferably 0.5-2mmol:1mmol:0.025-0.03mmol:0.75-2.1mmol:50mL, further preferably 1-1.5mmol:1mmol:0.026-0.028mmol:1-1.8mmol:50mL, and more preferably 1.25mmol:1mmol:0.027mmol:1.5mmol:50mL.
[0049] In the present invention, the concentration of the sodium borohydride solution in step 4) is preferably 0.05-0.2 mol / L, more preferably 0.08-0.18 mol / L, more preferably 0.1-0.15 mol / L; the rate of dropwise addition is preferably 0.5-2 mL / min, more preferably 0.8-1.8 mL / min, more preferably 1-1.5 mL / min; the molar ratio of sodium borohydride in the sodium borohydride solution to silver nitrate in the Pd-Ag mixed solution is preferably 8-10:1, more preferably 8.5-9.5:1, more preferably 9:1; the reaction is preferably carried out under stirring, and the stirring speed is preferably 500-700 rpm, more preferably 550-650 rpm, more preferably 600 rpm; the stirring time is preferably 0.5-2 h, more preferably 0.8-1.8 h, more preferably 1-1.5 h.
[0050] In the present invention, after the reaction in step 4) is completed, the silver palladium quantum dot anchored defect titanium dioxide nanoarray composite photocatalyst is preferably cleaned and dried, and the cleaning preferably includes deionized water cleaning and anhydrous ethanol cleaning in sequence, and the number of cleanings is independently preferably 2 to 4 times, and more preferably 3 times; the drying temperature is preferably 50 to 80°C, and more preferably 60 to 70°C; the drying time is preferably 10 to 14 hours, and more preferably 12 hours.
[0051] The present invention also provides a silver-palladium quantum dot anchored defective titanium dioxide nano-array composite photocatalyst prepared by the preparation method.
[0052] The present invention also provides the use of the silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst in degrading organic pollutants and disinfecting microorganisms.
[0053] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0054] Example 1
[0055] A titanium mesh of 5 cm × 3 cm, pore size of 2 × 4 mm, thickness of 0.5 mm was ultrasonically cleaned in deionized water at a frequency of 40 kHz for 15 min, in 1 mol / L hydrochloric acid at a frequency of 40 kHz for 10 min, in acetone at a frequency of 40 kHz for 15 min, and in anhydrous ethanol at a frequency of 40 kHz for 20 min. After cleaning, the titanium mesh was placed in a 60°C oven to dry for 30 min. The above operation was repeated for a titanium sheet of 5 cm × 3 cm.
[0056] The titanium mesh anode and the titanium sheet cathode (the distance between the positive and negative electrodes is 1.5 cm) were placed in a fluorinated ethylene glycol solution (the mass fraction of ammonium fluoride in the fluorinated ethylene glycol solution is 0.25%, and the mass fraction of water is 2%) at a temperature of 10°C, and anodized at a DC voltage of 55V for 4.5 hours. After the end, the DC voltage was directly adjusted to 10V, and a secondary anodization was performed for 5 minutes. After the secondary anodization, the titanium mesh was taken out and washed with deionized water 3 times and anhydrous ethanol 3 times in sequence. After washing, it was placed in a 60°C oven for drying for 30 minutes to obtain an amorphous titanium dioxide nanoarray.
[0057] The amorphous titanium dioxide nanoarrays were heated to 450°C at a rate of 2°C / min and annealed at 450°C for 2 h to obtain anatase titanium dioxide nanoarrays.
[0058] The titanium sheet was used as the anode and the anatase titanium dioxide nanoarray was used as the cathode (the distance between the anode and cathode plates was 1.5 cm). The temperature was 10°C and the formic acid aqueous solution (the volume fraction of formic acid in the formic acid aqueous solution was 8%) was 5 mA / cm 2 The cathode reduction was performed for 5 minutes. After the reduction was completed, the titanium dioxide nanoarray was taken out and washed with deionized water for 3 times and anhydrous ethanol for 3 times in sequence. After the washing was completed, it was placed in a 60° C. oven for drying for 60 minutes to obtain a defective titanium dioxide nanoarray rich in oxygen vacancies.
[0059] Palladium chloride and silver nitrate were dissolved in deionized water, and then polyvinyl pyrrolidone aqueous solution (polyvinyl pyrrolidone weight average molecular weight is 8000) and sodium citrate aqueous solution were added to prepare a Pd-Ag mixed solution (the molar volume ratio of palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water in the Pd-Ag mixed solution is 1.25mmol:1mmol:0.027mmol:1.5mmol:50mL). The Pd-Ag mixed solution was aerated at 600rpm under 5mL / min argon for 20min. The defective titanium dioxide nanoarrays rich in oxygen vacancies were placed vertically in the Pd-Ag mixed solution so that it was completely immersed, and argon was introduced at 5mL / min and stirred at 600rpm for 30min. 0.1 mol / L sodium borohydride aqueous solution was added dropwise at a rate of 1 mL / min. When the molar ratio of sodium borohydride to silver nitrate was 9:1, the addition was stopped. Argon was introduced at 5 mL / min and stirred at 600 rpm for 1 h to react. After being taken out, it was washed with deionized water 3 times and anhydrous ethanol 3 times in sequence, and dried in a vacuum oven at 60°C for 12 h to obtain a silver palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst, labeled as AgPd 1.25 / TiO 2 -4.5 composite photocatalyst.
[0060] Example 2
[0061] A titanium mesh of 5 cm × 3 cm, pore size of 2 × 4 mm, thickness of 0.5 mm was ultrasonically cleaned in deionized water at a frequency of 40 kHz for 10 min, in 1 mol / L hydrochloric acid at a frequency of 40 kHz for 15 min, in acetone at a frequency of 40 kHz for 20 min, and in anhydrous ethanol at a frequency of 40 kHz for 15 min. After cleaning, the titanium mesh was placed in a 50°C oven to dry for 40 min. The above operation was repeated for a titanium sheet of 5 cm × 3 cm.
[0062] The titanium mesh anode and the titanium sheet cathode (the distance between the positive and negative electrodes is 1 cm) were placed in a fluorinated ethylene glycol solution (the mass fraction of ammonium fluoride in the fluorinated ethylene glycol solution is 0.28%, and the mass fraction of water is 1.5%) at a temperature of 11°C, and anodized at a DC voltage of 45V for 2.5 hours. After the end, the DC voltage was directly adjusted to 13V, and a secondary anodization was performed for 6 minutes. After the secondary anodization, the titanium mesh was taken out and washed with deionized water twice and anhydrous ethanol twice in sequence. After washing, it was placed in an oven at 80°C and dried for 20 minutes to obtain an amorphous titanium dioxide nanoarray.
[0063] The amorphous titanium dioxide nanoarrays were heated to 480°C at a rate of 1.5°C / min and annealed at 480°C for 1.5 h to obtain anatase titanium dioxide nanoarrays.
[0064] With titanium sheet as anode and anatase titanium dioxide nanoarray as cathode (the distance between the anode and cathode plates is 1 cm), the ionization current was 4.5 mA / cm in a formic acid aqueous solution at 11°C (the volume fraction of formic acid in the formic acid aqueous solution was 6%). 2 The cathode reduction was performed for 8 minutes. After the reduction was completed, the titanium dioxide nanoarray was taken out, and it was washed twice with deionized water and twice with anhydrous ethanol in sequence. After the washing was completed, it was placed in a 50° C. oven to dry for 80 minutes to obtain a defective titanium dioxide nanoarray rich in oxygen vacancies.
[0065] Palladium chloride and silver nitrate were dissolved in deionized water, and then polyvinyl pyrrolidone aqueous solution (polyvinyl pyrrolidone weight average molecular weight is 8000) and sodium citrate aqueous solution were added to prepare a Pd-Ag mixed solution (the molar volume ratio of palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water in the Pd-Ag mixed solution is 1.5mmol:1mmol:0.026mmol:1.8mmol:50mL). The Pd-Ag mixed solution was aerated at 700rpm under 3mL / min argon for 10min. The defective titanium dioxide nanoarrays rich in oxygen vacancies were placed vertically in the Pd-Ag mixed solution so that it was completely immersed, and argon was introduced at 3mL / min and stirred at 500rpm for 40min. 0.18 mol / L sodium borohydride aqueous solution was added dropwise at a rate of 1.8 mL / min. When the molar ratio of sodium borohydride to silver nitrate was 8.5:1, the addition was stopped. Argon was introduced at 3 mL / min and stirred at 550 rpm for 1.8 h to react. After being taken out, it was washed twice with deionized water and twice with anhydrous ethanol, and dried in a vacuum oven at 80 °C for 10 h to obtain a silver palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst, labeled as AgPd 1.5 / TiO 2 -2.5 composite photocatalyst.
[0066] Example 3
[0067] A titanium mesh of 5 cm × 3 cm, pore size of 2 × 4 mm, and thickness of 0.5 mm was ultrasonically cleaned in deionized water at a frequency of 40 kHz for 10 min, in 1 mol / L hydrochloric acid at a frequency of 40 kHz for 15 min, in acetone at a frequency of 40 kHz for 10 min, and in anhydrous ethanol at a frequency of 40 kHz for 20 min. After cleaning, the titanium mesh was placed in an oven at 80°C for 20 min. The above operation was repeated for a titanium sheet of 5 cm × 3 cm.
[0068] The titanium mesh anode and the titanium sheet cathode (the distance between the positive and negative electrodes is 2 cm) were placed in a fluorinated ethylene glycol solution (the mass fraction of ammonium fluoride in the fluorinated ethylene glycol solution is 0.22%, and the mass fraction of water is 2.5%) at a temperature of 9°C, and anodized at a DC voltage of 50V for 3.5 hours. After the end, the DC voltage was directly adjusted to 8V, and a secondary anodization was performed for 8 minutes. After the secondary anodization, the titanium mesh was taken out and washed with deionized water 4 times and anhydrous ethanol 4 times in sequence. After washing, it was placed in a 50°C oven for 40 minutes to obtain an amorphous titanium dioxide nanoarray.
[0069] The amorphous titanium dioxide nanoarray was heated to 430°C at a rate of 2.5°C / min and annealed at 430°C for 2.5h to obtain anatase titanium dioxide nanoarray.
[0070] The titanium sheet was used as the anode and the anatase titanium dioxide nanoarray was used as the cathode (the distance between the anode and cathode plates was 2 cm). The sample was placed in a formic acid aqueous solution at a temperature of 9°C (the volume fraction of formic acid in the formic acid aqueous solution was 9%) at a current of 5.5 mA / cm 2 The cathode reduction was performed for 4 minutes. After the reduction was completed, the titanium dioxide nanoarray was taken out and washed with deionized water 4 times and anhydrous ethanol 4 times in sequence. After the washing was completed, it was placed in an oven at 80° C. and dried for 50 minutes to obtain a defective titanium dioxide nanoarray rich in oxygen vacancies.
[0071] Palladium chloride and silver nitrate were dissolved in deionized water, and then polyvinyl pyrrolidone aqueous solution (polyvinyl pyrrolidone weight average molecular weight is 8000) and sodium citrate aqueous solution were added to prepare a Pd-Ag mixed solution (the molar volume ratio of palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water in the Pd-Ag mixed solution is 1mmol:1mmol:0.028mmol:1mmol:50mL). The Pd-Ag mixed solution was aerated at 500rpm under 8mL / min argon for 30min. The defective titanium dioxide nanoarrays rich in oxygen vacancies were placed vertically in the Pd-Ag mixed solution so that it was completely immersed, and argon was introduced at 8mL / min and stirred at 700rpm for 20min. 0.08 mol / L sodium borohydride aqueous solution was added dropwise at a rate of 0.8 mL / min. When the molar ratio of sodium borohydride to silver nitrate was 9.5:1, the addition was stopped. Argon was introduced at 8 mL / min and stirred at 650 rpm for 0.8 h to react. After being taken out, it was washed with deionized water 4 times and anhydrous ethanol 4 times in sequence, and dried in a vacuum oven at 50 °C for 14 h to obtain a silver palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst, labeled as AgPd / TiO 2 -3.5 composite photocatalyst.
[0072] 2.5×1.5 cm of AgPd / TiO prepared in Example 3 were placed 2 -3.5 Composite photocatalyst, TiO 2 The catalyst was added to 30 mL of a 20 ppm tetracycline hydrochloride aqueous solution to obtain a mixed solution, the temperature of the mixed solution was controlled to 25°C, and the solution to be tested was obtained by stirring at 100 rpm for 30 min in a dark environment. The solution to be tested was controlled at 25°C, placed under a 300 W xenon lamp (wavelength>420 nm) with a filter, and continuously stirred at 100 rpm. Every 20 min, 3 mL was removed from the solution to be tested and placed in a centrifuge, centrifuged at 1000 rpm for 5 min, and the supernatant was taken. The absorbance at 356 nm was measured using a UV-visible spectrophotometer, and the concentration of tetracycline hydrochloride in the solution to be tested was calculated to obtain AgPd / TiO 2 -3.5 Composite photocatalyst and TiO 2 The photodegradation rate of tetracycline hydrochloride by the catalyst, such as Figure 4 , 5 shown.
[0073] Depend on Figure 4 , 5 It can be seen that after 100 min of degradation, AgPd / TiO 2 -3.5 composite photocatalyst photodegradation rate of tetracycline hydrochloride reached 93.22%, which was higher than that of TiO 2 The photodegradation rate of the catalyst increased by 5.38 times.
[0074] 2.5×1.5 cm of AgPd / TiO prepared in Example 3 were placed 2 -3.5 Composite photocatalyst, TiO 2 The catalyst was added to 30 mL of a 12 ppm ciprofloxacin aqueous solution to obtain a mixed solution, the temperature of the mixed solution was controlled to 25°C, and the solution to be tested was obtained by stirring at 100 rpm for 30 min in a dark environment. The solution to be tested was controlled at 25°C, placed under a 300 W xenon lamp (wavelength>420 nm) with a filter, and continuously stirred at 100 rpm. Every 20 min, 3 mL was removed from the solution to be tested and placed in a centrifuge, centrifuged at 1000 rpm for 100 min, and the supernatant was taken. The absorbance at 278 nm was measured using a UV-visible spectrophotometer, and the concentration of ciprofloxacin in the solution to be tested was calculated to obtain AgPd / TiO 2 -3.5 Composite photocatalyst and TiO 2 The photodegradation rate of ciprofloxacin by the catalyst, such as Figure 6 , 7 shown.
[0075] Depend on Figure 6 ,7 It can be seen that after 100 min of degradation, AgPd / TiO 2 The photodegradation rate of ciprofloxacin by the composite photocatalyst of -3.5 reached 84.11%, which was higher than that of TiO 2 The photodegradation rate of the catalyst increased by 5.78 times.
[0076] 2.5×1.5 cm of AgPd / TiO prepared in Example 3 were placed 2 -3.5 Composite photocatalyst, TiO 2 The colony density when the catalyst is added to 30 mL is 7.3 log 10 (cfu / mL) of Escherichia coli solution to obtain a mixed bacterial solution, control the temperature of the mixed bacterial solution to 25°C, and stir at a speed of 100rpm for 30min in a dark environment to obtain a test bacterial solution. The test bacterial solution was controlled at 25°C, placed under a 300W xenon lamp (wavelength>420nm) with a filter, and continuously stirred at a speed of 100rpm. Every 40min, 10μL of the bacterial solution was transferred from the test bacterial solution, diluted 100 times with distilled water, and then spread on a nutrient agar medium (the composition of the nutrient agar medium is peptone 10.0g / L, beef powder 3.0g / L, sodium chloride 5.0g / L, agar 15.0g / L), and then transferred to a 36°C shaker and cultured at a constant temperature of 180rpm for 24h to observe the survival of Escherichia coli, such as Figure 8 , 9 shown.
[0077] Depend on Figure 8 , 9 It can be seen that after 200 minutes of disinfection, AgPd / TiO 2 -3.5 composite photocatalyst can completely inactivate Escherichia coli, and the photokilling rate of Escherichia coli is significantly better than that of TiO 2 catalyst.
[0078] 2.5×1.5 cm of AgPd / TiO prepared in Example 3 were placed 2 -3.5 Composite photocatalyst, TiO 2 The colony density when the catalyst is added to 30 mL is 7.5 log 10(cfu / mL) of white Staphylococcus aureus solution was added to obtain a mixed bacterial solution, the temperature of the mixed bacterial solution was controlled to 25°C, and the mixture was stirred at a speed of 100 rpm for 30 minutes in a dark environment to obtain the test bacterial solution. The test bacterial solution was controlled at 25°C, placed under a 300W xenon lamp (wavelength>420nm) with a filter, and continuously stirred at a speed of 100 rpm. 10 μL of bacterial solution was transferred from the test bacterial solution every 40 minutes, diluted 100 times with distilled water, and then spread on a nutrient agar medium (the composition of the nutrient agar medium is peptone 10.0 g / L, beef powder 3.0 g / L, sodium chloride 5.0 g / L, agar 15.0 g / L), and then transferred to a 36°C shaker and cultured at a constant temperature of 180 rpm for 24 hours to observe the survival of white Staphylococcus aureus, such as Fig.10 , 11 shown.
[0079] Depend on Fig.10 , 11 It can be seen that after 200 minutes of disinfection, AgPd / TiO 2 -3.5 composite photocatalyst has a photo-disinfecting rate of no less than 50% for Staphylococcus aureus, which is significantly better than TiO 2 catalyst.
[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a composite photocatalyst of silver-palladium quantum dots anchoring defective titanium dioxide nanoarrays, It is characterized in that The following steps are included: 1) Anodizing the titanium sheet cathode and the titanium mesh anode in a fluorinated ethylene glycol solution to obtain an amorphous titanium dioxide nanoarray; 2) annealing the amorphous titanium dioxide nanoarray to obtain anatase titanium dioxide nanoarray; 3) using the titanium sheet as an anode and the anatase titanium dioxide nanoarray as a cathode, and performing cathode reduction in a formic acid solution to obtain a defective titanium dioxide nanoarray; 4) Under an argon atmosphere, the defective titanium dioxide nanoarray is placed in a Pd-Ag mixed solution, and a sodium borohydride solution is added dropwise to the Pd-Ag mixed solution for reaction, thereby obtaining a silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst.
2. The preparation method according to claim 1, It is characterized in that Step 1) The temperature of the anodization is 8-12° C., and the distance between the anodized plates is 1-2 cm. The anodization is performed twice, the voltage of the first anodization is 45-55 V, and the time is 2.5-4.5 h; the voltage of the second anodization is 5-15 V, and the time is 3-10 min.
3. The preparation method according to claim 1 or 2, It is characterized in that Step 1) The fluorinated ethylene glycol solution comprises ammonium fluoride, ethylene glycol and water; the mass fraction of ammonium fluoride in the fluorinated ethylene glycol solution is 0.2-0.3%, and the mass fraction of water is 1-3%.
4. The preparation method according to claim 3, It is characterized in that Step 2) The annealing temperature is 400-500° C., the annealing time is 1-3 hours, and the annealing heating rate is 1-3° C. / min.
5. The preparation method according to claim 4, It is characterized in that Step 3) The temperature of the cathode reduction is 8-12°C, the distance between the cathode reduction plates is 1-2 cm, and the current density of the cathode reduction is 4-6 mA / cm 2 The cathode reduction time is 3 to 10 minutes, and the volume fraction of formic acid in the formic acid solution is 5 to 10%.
6. The preparation method according to claim 4 or 5, It is characterized in that Step 4) The Pd-Ag mixed solution comprises palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water, and the molar volume ratio of palladium chloride, silver nitrate, polyvinyl pyrrolidone, sodium citrate and water is 0.5-2mmol:1mmol:0.025-0.03mmol:0.75-2.1mmol:50mL.
7. The preparation method according to claim 6, It is characterized in that Step 4) The concentration of the sodium borohydride solution is 0.05-0.2 mol / L, the rate of addition is 0.5-2 mL / min, the molar ratio of sodium borohydride in the sodium borohydride solution to silver nitrate in the Pd-Ag mixed solution is 8-10:1; the reaction is carried out under stirring conditions, the stirring speed is 500-700 rpm, and the stirring time is 0.5-2 h.
8. Silver-palladium quantum dot-anchored defective titanium dioxide nanoarray composite photocatalyst prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the silver-palladium quantum dot anchored defective titanium dioxide nanoarray composite photocatalyst as described in claim 8 in degrading organic pollutants and disinfecting microorganisms.
Citation Information
Patent Citations
Method for performing photoelectrolysis of water and preparing hydrogen by using palladium quantum dot modified titanium dioxide nanotube array
CN102226284A
Preparation method of Ag2O quantum dot hybrid ZnIn2S4 nanosheet p-n type composite photocatalyst
CN109395744A
Silver-loaded titanium dioxide nano array composite thin film, preparing method and application of thin film in trace substance detection
CN109655443A
Bimetallic cluster supported photocatalyst, preparation method and application
CN110302780A
Methods to fabricate vertically oriented anatase nanowire arrays on transparent conductive substrates and applications thereof
US20130048947A1
Cited By
Rare noble metal / Ti (at) TiO2-x self-supporting gas purification material, preparation and application thereof and air purifier
CN120771858A
Rare and precious metals / Ti@TiO 2-x Self-supporting gas purification materials, their preparation, application, and air purifiers
CN120771858B