Thermal cracking carbon black supported metal catalyst as well as preparation method and application thereof

By thermally cracking carbon black-loaded nickel or nickel-ruthenium bimetallic catalyst, the problem of disposing of high oil content wastewater during thermal cracking of waste tires is solved, efficient catalytic gasification is achieved, and the degradation rate and hydrogen yield are significantly improved, avoiding the high catalyst cost. Problem, "using waste to control waste" and closed-loop treatment of pollutants has been achieved.

CN118988323APending Publication Date: 2024-11-22QINGDAO IXIDA RENEWABLE RESOURCES CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411092542.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

It is difficult to dispose of high oil-containing wastewater generated during thermal cracking of waste tires. The prior art uses supercritical water oxidation to degrade organic matter in water while achieving inefficiency of hydrogen-rich gas in the absence of a catalyst. How to control the cost of catalyst It is key to achieving efficient catalytic gasification under the slightest.

Method used

Thermal cracking carbon black-supported nickel or nickel and ruthenium bimetallic catalyst is prepared by co-precipitation method, and is used to prepare hydrogen-rich gas for catalytic gasification of oil-containing wastewater, achieving efficient degradation of organic matter and producing high-quality hydrogen-rich clean fuel.

Benefits of technology

While reducing the risk of pollution, it effectively degrades the total organic carbon in oil-containing wastewater, and the hydrogen yield and methane selectivity are significantly improved, and the total organic carbon degradation rate reaches 72% to 98%, avoiding the high cost of traditional catalysts and achieving "Treat waste with waste" and closed-loop treatment of pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a thermal cracking carbon black supported metal catalyst as well as a preparation method and application thereof, and belongs to the technical field of organic waste recycling. The thermal cracking carbon black supported metal catalyst is prepared by taking deashing thermal cracking carbon black as a carrier and loading nickel or nickel and ruthenium bimetals by adopting a coprecipitation method. The catalyst provided by the invention is mainly applied to preparation of hydrogen-rich gas by catalytic gasification of oil-containing wastewater, and can degrade 98% of total organic carbon in the wastewater under the condition of catalytic gasification, so that high-quality hydrogen-rich clean fuel is produced while the pollution risk is reduced, and waste is turned into wealth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of organic waste resource utilization, and in particular relates to a thermal cracking carbon black-loaded metal catalyst and a preparation method and application thereof, in particular, application in catalytic gasification of oily wastewater to prepare hydrogen-rich gas. Background Art

[0002] The main component of waste tires is rubber, which is a high molecular organic matter. Improper disposal of waste tires not only causes environmental pollution but also wastes resources. Pyrolysis, as a "bottom-line" disposal method for waste tires, is the preferred method to achieve "reduction, harmlessness, resource utilization, and stabilization" of waste tires. After pyrolysis, waste tires can produce pyrolysis carbon black, pyrolysis oil, steel wire, and pyrolysis gas. The re-entry of these products into the market can significantly reduce the dependence of related industries on fossil energy.

[0003] However, during the thermal cracking of waste tires, the surface moisture of the raw materials cannot be completely removed. The condensation of hydrogen and oxygen bonds during the cracking of rubber macromolecules will also produce a certain amount of water molecules. These water molecules enter the oil storage tank together with the cracked oil and gas products, and settle as oily wastewater after standing. The disposal of wastewater with high oil content is extremely difficult and poses a serious threat to nearby water and land resources. This is contrary to the original intention of "harmless disposal" of waste tires. Therefore, it is of great significance to treat the high organic matter content wastewater generated during the thermal cracking of waste tires on site.

[0004] Supercritical water oxidation is a process of oxidative degradation of organic waste using water as a medium at a temperature and pressure above the critical point of water (374.3°C and 22.12MPa). This technology is a clean, pollution-free, and environmentally friendly organic waste treatment technology, and the final emissions are CO2, H2O, N2, etc., which will not cause secondary pollution. Supercritical water oxidation can completely and thoroughly destroy the structure of organic matter, has a good degradation effect on alcohol, phenol, benzene, nitrogen and sulfur components in sewage, and can complete the reaction in a very short time. However, in the absence of a catalyst, it is inefficient to degrade organic matter in water and simultaneously achieve hydrogen-rich gas through supercritical water oxidation technology. Therefore, how to achieve efficient catalytic gasification of oily wastewater while controlling the cost of the catalyst is the key to expanding the prospects of this technology. Summary of the invention

[0005] The present invention provides a thermal cracking carbon black-loaded metal catalyst and a preparation method and application thereof. The catalyst uses thermal cracking carbon black as a catalyst carrier and non-precious metals as a main catalyst. The catalyst can be applied to the catalytic gasification of oily wastewater to prepare hydrogen-rich gas. While reducing the risk of pollution, high-quality hydrogen-rich clean fuel can be produced, thus turning waste into treasure.

[0006] In order to achieve the above object, the present invention provides a thermal cracking carbon black loaded metal catalyst, which is prepared by loading nickel, or nickel and ruthenium bimetallic by coprecipitation method using deashed thermal cracking carbon black as a carrier.

[0007] Preferably, the nickel loading is 1 to 5 wt.%, and the Ru loading is 0 to 5 wt.%.

[0008] Preferably, the coprecipitation method is adopted to prepare the bimetallic material by loading nickel and ruthenium, which comprises the following steps:

[0009] According to the bimetallic loading, nickel nitrate or nickel nitrate and ruthenium trichloride hexahydrate are weighed and mixed evenly in deionized water to obtain a mixed solution;

[0010] The mixed solution is mixed with the deashing thermal cracking carbon black and stirred, and during the stirring process, an alkali solution (such as NaOH) with a concentration of 10 to 30 wt.% is added to precipitate the metal salt and fully and evenly combine with the deashing thermal cracking carbon black to form a solid mixture;

[0011] The solid mixture is separated from the solution, washed with water until pH=7, and then the solid particles are calcined at 600-800°C in a nitrogen atmosphere for 3-5 hours, and then cooled to obtain a bimetallic catalyst.

[0012] In the above scheme, the obtained bimetallic catalyst needs to be activated within 24 hours before use. For example, it can be activated at 300-450°C for 2-4 hours in an atmosphere of a mixture of H2 and N2 with a flow rate of 2:8, and then placed in a vacuum desiccator for proper storage.

[0013] Preferably, the deashing thermal cracking carbon black is prepared by the following method:

[0014] 3M nitric acid solution and 3M hydrofluoric acid solution with a mass of 10 times that of carbon black were used successively at 80-120°C for 3h, and after solid-liquid separation, the solid product was washed to pH = 7;

[0015] The deashed thermal cracking carbon black after the acid treatment is dried, fully ground and mixed with the same mass of KOH, and placed in a tube furnace and calcined in a nitrogen atmosphere;

[0016] The calcined product was treated with 10 times the mass of 30% nitric acid solution by stirring for 3 hours, and after solid-liquid separation, it was washed with water until pH = 7 to obtain deashed thermal cracking carbon black.

[0017] The present invention also provides a method for preparing hydrogen-rich gas from oily wastewater using the pyrolysis carbon black-loaded metal catalyst described in any of the above technical solutions, comprising the following steps:

[0018] The oily wastewater is loaded into the reactor, and the thermal cracking carbon black-loaded metal catalyst is added and then sealed, and the gas in the reactor is evacuated with nitrogen and then a catalytic gasification reaction is carried out;

[0019] After the reaction is completed, the reactor is cooled to room temperature, the gaseous product is collected, the catalyst and the reaction liquid are centrifuged, the aqueous phase product is collected and the catalyst is recovered;

[0020] After treatment, the total organic carbon in the aqueous phase product is degraded by 72% to 98% compared with that in the raw oily wastewater.

[0021] Preferably, the loading amount of the oily wastewater in the reactor is 10% to 25% of the reactor capacity, and the amount of catalyst added is 5% to 20% of the total organic carbon mass in the oily wastewater.

[0022] Preferably, the reactor is an intermittent stainless steel reactor, the catalytic gasification reaction temperature is 400-700° C., the pressure is 12-45 MPa, and the reaction time is 15-90 min.

[0023] As a preferred embodiment, the oily wastewater is the oily wastewater naturally precipitated from the oil tank of the waste tire thermal cracking plant, with TOC ≥ 26g / L;

[0024] Thermal cracking carbon black is taken from the solid product after the cracking process of the waste tire thermal cracking factory. After grinding, the product particle size is ≥1200 mesh.

[0025] The present invention also provides an application of the thermal cracking carbon black-loaded metal catalyst according to any of the above technical solutions in the catalytic gasification of oily wastewater to prepare hydrogen-rich gas.

[0026] Preferably, under supercritical catalytic gasification conditions, the total organic carbon in the oily wastewater is degraded to 98%, the hydrogen yield is 2.57 mmol / mL wastewater, the methane yield is 2.02 mmol / mL wastewater, and the methane selectivity is 91.71%.

[0027] Compared with the prior art, the advantages and positive effects of the present invention are:

[0028] 1. The present invention uses thermal cracking carbon black as a catalyst carrier and non-precious metals as the main catalyst, which not only realizes the high value and harmless treatment of thermal cracking solid products, realizes "waste treatment with waste", but also effectively controls the catalyst cost, avoiding the high catalyst cost problem caused by the use of metal oxides to load precious metals in traditional critical water catalytic gasification technology;

[0029] 2. The present invention utilizes the prepared pyrolysis carbon black loaded metal catalyst to catalytically gasify the oily wastewater generated in the pyrolysis process to prepare hydrogen-rich gas, and does not use any added substances in the reaction process, thereby avoiding the introduction of new pollution sources and reducing the related consumables required for the catalytic reaction, thereby achieving on-site disposal and closed-loop treatment of pollutants in the waste tire pyrolysis plant area;

[0030] 3. When the catalyst of the present invention is used for catalytic gasification of oily wastewater to prepare hydrogen-rich gas, it can significantly reduce the total organic carbon in the oily wastewater while obtaining hydrogen-rich combustible gas with high added value, that is, the degradation rate of the total organic carbon in the organic wastewater reaches more than 72%, and can reach up to 98%, and the gas product has high selectivity for hydrogen and methane. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.013g of a catalyst with a nickel loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0034] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 72.87% compared with the raw material, the hydrogen yield was 1.67 mmol / mL wastewater, the methane yield was 1.34 mmol / mL wastewater, and the methane selectivity was 60.84%.

[0035] Example 2

[0036] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.026g of a catalyst with a nickel loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0037] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 84.34% compared with the raw material, the hydrogen yield was 1.73 mmol / mL wastewater, the methane yield was 1.68 mmol / mL wastewater, and the methane selectivity was 76.28%.

[0038] Example 3

[0039] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0040] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 87.48% compared with the raw material, the hydrogen yield was 1.78 mmol / mL wastewater, the methane yield was 1.73 mmol / mL wastewater, and the methane selectivity was 78.55%.

[0041] Example 4

[0042] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.052g of a catalyst with a nickel loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0043] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 87.82% compared with the raw material, the hydrogen yield was 1.66 mmol / mL wastewater, the methane yield was 1.72 mmol / mL wastewater, and the methane selectivity was 78.09%.

[0044] Example 5

[0045] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) was loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 5wt.% and a ruthenium loading of 1wt.% was added, the flange was sealed, and the gas in the reactor was evacuated with nitrogen; the sealed reactor was subjected to catalytic gasification reaction at 600°C for 30min; after the reaction, the reactor was cooled to room temperature, the gaseous products were collected, the catalyst and the reaction liquid phase were centrifuged, and the liquid products were collected; the catalyst was fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0046] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 98.03% compared with the raw material, the hydrogen yield was 2.41 mmol / mL wastewater, the methane yield was 2.01 mmol / mL wastewater, and the methane selectivity was 91.26%.

[0047] Example 6

[0048] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) was loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 3wt.% and a ruthenium loading of 3wt.% was added, the flange was sealed, and the gas in the reactor was evacuated with nitrogen; the sealed reactor was subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor was cooled to room temperature, the gaseous products were collected, the catalyst and the reaction liquid were centrifuged, and the liquid products were collected; the catalyst was fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0049] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 97.50% compared with the raw material, the hydrogen yield was 2.57 mmol / mL wastewater, the methane yield was 2.02 mmol / mL wastewater, and the methane selectivity was 91.71%.

[0050] Example 7

[0051] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 1wt.% and a ruthenium loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction is completed, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0052] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 98.11% compared with the raw material, the hydrogen yield was 2.54 mmol / mL wastewater, the methane yield was 1.98 mmol / mL wastewater, and the methane selectivity was 89.90%.

[0053] Example 8

[0054] Catalytic gasification uses a 100mL stainless steel reactor. 10mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 1wt.% and a ruthenium loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 400°C for 15min; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0055] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 80.97% compared with the raw material, the hydrogen yield was 1.42 mmol / mL wastewater, the methane yield was 1.31 mmol / mL wastewater, and the methane selectivity was 59.48%.

[0056] Example 9

[0057] Catalytic gasification uses a 100mL stainless steel reactor. 25mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 1wt.% and a ruthenium loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 500°C for 60min; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0058] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 82.37% compared with the raw material, the hydrogen yield was 1.52 mmol / mL wastewater, the methane yield was 1.47 mmol / mL wastewater, and the methane selectivity was 66.74%.

[0059] Example 10

[0060] Catalytic gasification uses a 100mL stainless steel reactor. 20mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, 0.039g of a catalyst with a nickel loading of 1wt.% and a ruthenium loading of 5wt.% is added, the flange is sealed, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 700°C for 90 minutes; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0061] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 86.19% compared with the raw material, the hydrogen yield was 1.69 mmol / mL wastewater, the methane yield was 1.75 mmol / mL wastewater, and the methane selectivity was 79.46%.

[0062] Comparative Example 1

[0063] Catalytic gasification uses a 100mL stainless steel reactor. 25mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 400°C for 15 minutes; after the reaction, the reactor is cooled to room temperature, the gaseous products are collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid products are collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0064] After analyzing the total organic carbon (TOC) of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 42.30% compared with the raw material, the hydrogen yield was 0.52 mmol / mL wastewater, the methane yield was 0.67 mmol / mL wastewater, and the methane selectivity was 30.42%.

[0065] Comparative Example 2

[0066] Catalytic gasification uses a 100mL stainless steel reactor. 25mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 15 minutes; after the reaction, the reactor is cooled to room temperature, the gas product is collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid product is collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0067] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 48.69% compared with the raw material, the hydrogen yield was 0.61 mmol / mL wastewater, the methane yield was 0.89 mmol / mL wastewater, and the methane selectivity was 40.41%.

[0068] Comparative Example 3

[0069] Catalytic gasification uses a 100mL stainless steel reactor. 25mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor is cooled to room temperature, the gas product is collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid product is collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0070] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 56.53% compared with the raw material, the hydrogen yield was 0.88 mmol / mL wastewater, the methane yield was 1.01 mmol / mL wastewater, and the methane selectivity was 45.86%.

[0071] Comparative Example 4

[0072] Catalytic gasification uses a 100mL stainless steel reactor. 15mL of oily wastewater (TOC: 26.43g / L) is loaded into an intermittent stainless steel reactor, and the gas in the reactor is evacuated with nitrogen; the sealed reactor is subjected to catalytic gasification reaction at 600°C for 30 minutes; after the reaction, the reactor is cooled to room temperature, the gas product is collected, the catalyst and the reaction liquid phase are centrifuged, and the liquid product is collected; the catalyst is fully washed with deionized water and ethanol, fully dried at 70°C, and stored in a vacuum dryer;

[0073] After analyzing the TOC of the aqueous phase and performing TCD detection on the gas phase, the TOC degradation efficiency and the hydrogen and methane yields were obtained, and the results are listed in Table 1; among them, after the catalytic gasification reaction, the total organic carbon of the aqueous phase product was reduced by 65.34% compared with the raw material, the hydrogen yield was 1.13 mmol / mL wastewater, the methane yield was 1.12 mmol / mL wastewater, and the methane selectivity was 50.85%.

[0074] The reaction conditions, component ratios and test results of the above examples and comparative examples are shown in Table 1.

[0075] Table 1 Wastewater TOC removal efficiency and hydrogen-rich gas yield under different reaction conditions

[0076]

[0077] In the above table, the units of each parameter are as follows: temperature: ℃, time: min, loading: mL, catalyst loading: 100% g / gTOC, loading: wt.%, TOC: g / L, TOC degradation efficiency: %, yield: mmol / mL wastewater, CH4 selectivity: %.

[0078] In addition, compared with the comparative patent (patent number: CN201080027544.7), this catalyst uses thermal cracking carbon black as a carrier to achieve "waste treatment with waste" and avoid the additional cost of the catalytic process; the highest carbon conversion efficiency of the catalyst described in the comparative patent is 85.39%, which is much lower than the carbon conversion efficiency described in this patent (98.11%). The comparative patent (patent number: CN201410397793.5) uses the precious metal Ru as the main active component, and the conversion rate of phenol is less than 80%, which is lower than the catalyst economy and the degradation efficiency of the target reactant than the case reported.

[0079] Compared with the control example (TOC degradation efficiency: 42.30-65.34%; methane selectivity: 30.42-50.85%), the catalyst loaded with thermal cracking carbon black has significantly improved catalytic degradation efficiency of organic matter in oily wastewater and methane selectivity of gas product (TOC degradation efficiency: 72.87-98.11%; methane selectivity: 60.84-91.71%). In addition, Ru, as a precious metal, can achieve a good catalytic effect with a loading of only 1wt.%.

Claims

1. A thermal cracking carbon black supported metal catalyst, characterized in that: The deashing thermal cracking carbon black is used as a carrier and prepared by a co-precipitation method through loading nickel or nickel and ruthenium bimetallic.

2. The thermal cracking carbon black supported metal catalyst according to claim 1, characterized in that: The nickel loading is 1-5 wt.%, and the Ru loading is 0-5 wt.%.

3. The thermal cracking carbon black supported metal catalyst according to claim 1, characterized in that: The co-precipitation method is used to prepare the nickel and ruthenium bimetallic material, which includes the following steps: According to the bimetallic loading, nickel nitrate or nickel nitrate and ruthenium trichloride hexahydrate are weighed and mixed evenly in deionized water to obtain a mixed solution; The mixed solution is mixed with the deashing thermal cracking carbon black and stirred, and during the stirring process, an alkali solution with a concentration of 10 to 30 wt.% is added to precipitate the metal salt and fully and evenly combine with the deashing thermal cracking carbon black to form a solid mixture; The solid mixture is separated from the solution, washed with water until pH=7, and then the solid particles are calcined at 600-800°C in a nitrogen atmosphere for 3-5 hours, and then cooled to obtain a bimetallic catalyst.

4. The thermal cracking carbon black supported metal catalyst according to claim 1, characterized in that: Deashed thermal cracking carbon black is prepared by the following method: 3M nitric acid solution and 3M hydrofluoric acid solution with a mass of 10 times that of carbon black were used successively at 80-120°C for 3h, and after solid-liquid separation, the solid product was washed to pH = 7; The deashed thermal cracking carbon black after the acid treatment is dried, fully ground and mixed with the same mass of KOH, and placed in a tube furnace and calcined in a nitrogen atmosphere; The calcined product was treated with 10 times the mass of 30% nitric acid solution by stirring for 3 hours, and after solid-liquid separation, it was washed with water until pH = 7 to obtain deashed thermal cracking carbon black.

5. A method for preparing hydrogen-rich gas from oily wastewater using the pyrolysis carbon black-supported metal catalyst according to any one of claims 1 to 4, characterized in that: The following steps are involved: The oily wastewater is loaded into the reactor, and the thermal cracking carbon black-loaded metal catalyst is added and then sealed, and the gas in the reactor is evacuated with nitrogen and then a catalytic gasification reaction is carried out; After the reaction is completed, the reactor is cooled to room temperature, the gaseous product is collected, the catalyst and the reaction liquid are centrifuged, the aqueous phase product is collected and the catalyst is recovered; After treatment, the total organic carbon in the aqueous phase product is degraded by 72% to 98% compared with that in the raw oily wastewater.

6. The method according to claim 5, characterized in that The loading amount of the oily wastewater in the reactor is 10% to 25% of the reactor capacity, and the added amount of the catalyst is 5% to 20% of the total organic carbon mass in the oily wastewater.

7. The method according to claim 5, characterized in that The reactor is an intermittent stainless steel reactor, the catalytic gasification reaction temperature is 400-700° C., and the reaction time is 15-90 minutes.

8. The method according to any one of claims 5 to 7, characterized in that: The oily wastewater is the oily wastewater naturally precipitated from the oil tank of the waste tire thermal cracking plant, with TOC ≥ 26g / L; Thermal cracking carbon black is taken from the solid product after the cracking process of the waste tire thermal cracking factory. After grinding, the product particle size is ≥1200 mesh.

9. Use of the thermal cracking carbon black-supported metal catalyst according to any one of claims 1 to 4 in catalytic gasification of oily wastewater to produce hydrogen-rich gas.

10. The use according to claim 9, characterized in that: Under supercritical catalytic gasification conditions, the total organic carbon in the oily wastewater was degraded to 98%, the hydrogen yield reached 2.57 mmol / mL wastewater, the methane yield reached 2.02 mmol / mL wastewater, and the methane selectivity reached 91.71%.

Citation Information

Cited By

  • Catalyst taking thermal cracking carbon black as carrier as well as preparation method and application of catalyst

    CN120861087A

  • High-salinity wastewater double-oxidation treatment system and method

    CN120964972A