Preparation method of Na < + >-Cu / SiO2 catalyst applied to PET plastic degradation
Through the preparation method of Na+-Cu/SiO2 catalyst, combined with hydrothermal and two-step annealing technology, the problems of catalyst dissolution and environmental pollution in PET plastic degradation are solved, efficient and safe PET degradation are achieved, and new PET degradation is provided. Ideas.
Patent Information
- Application Number
- CN202411055615.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-22
AI Technical Summary
The existing PET plastic degradation catalysts have problems such as difficulty in dissolution, limited catalytic effect, high reaction temperature, long time, high cost and environmental pollution. In particular, precious metal catalysts are prone to explosion and produce highly toxic xylene products in the hydrogenation reaction.
Using the preparation method of Na+-Cu/SiO2 catalyst, the Na+ ions are introduced to regulate the Cu atomic position by combining hydrothermal and two-step annealing, and the selectivity and activity of the catalyst are improved, and the quantitative conversion of PET is achieved through methanol alcoholylation reaction. The product is separated by distillation by paraxylene and ethylene glycol, and the use of hydrogen reaction is avoided.
It realizes the maintenance of catalyst activity and stability under high temperature and high pressure, converts PET into paraxylene and ethylene glycol at low cost, avoids the dissolution of traditional catalysts and environmental pollution problems, and provides efficient, safe and environmentally friendly methods for PET degradation. .
Smart Images

Figure CN118988326A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling and reusing packaging waste, and more specifically, to a method for preparing a Na+-Cu / SiO2 catalyst used in the degradation of PET plastics. Background Art
[0002] PET has excellent mechanical properties, anti-friction properties, anti-creep properties, rigidity, hardness, etc., and is non-toxic and tasteless, has good transparency, and is light in weight. It is widely used in food packaging, beverage bottles, fibers, and films. The widespread use of PET also causes a large amount of solid waste every year, and these solid wastes are difficult to degrade naturally, causing great damage to the environment. At present, the methods for recycling and degradation of PET mainly include physical methods, chemical methods, and biological methods. However, since PET is chemically inert and it is difficult to rely on air or microorganisms to degrade naturally, the current research is more about the physical recycling and degradation method and chemical recycling and degradation method of PET. Common physical recycling treatment methods mainly include mixing, dissolving, melting, granulation and other means, which are suitable for recycling materials with fewer impurities, but the mechanical properties of PET will change greatly during the mechanical regeneration process. Chemical recycling treatment methods mainly include hydrolysis, glycolysis, aminolysis and other processes to completely or partially depolymerize PET polymers into monomers / oligomers and other chemical substances.
[0003] The alcoholysis of PET is the most studied method. The alcohols used include methanol, diols, fatty alcohols and other polyols. Different alcoholysis agents are selected, and the products after degradation will also be different. Among them, the methanol depolymerization method uses methanol as a solvent under certain operating conditions and adds a certain amount of catalyst to degrade PET into ethylene glycol and ethylene terephthalate. Its catalyst plays an irreplaceable role in this reaction, and the type of catalyst has a direct relationship with the degradation effect. At present, the catalysts used for PET alcoholysis mainly include metal salt catalysts, heterogeneous catalysts, ionic liquid catalysts, etc. Metal salt catalysts have a significant catalytic effect in PET degradation reactions, but this type of catalyst is easily soluble in ethylene glycol and is difficult to separate from the mixture after the reaction. Although heterogeneous catalysts can be separated from the product, due to their small specific surface area, the catalytic effect is limited, and the temperature required for the catalytic reaction is extremely high. Although ionic liquid catalysts reduce the requirements for reaction temperature, from the perspective of catalytic effect, the reaction time is long, and the monomer yield is extremely low. In addition, the price of ionic liquids is relatively expensive, and it is difficult to achieve industrial application.
[0004] In view of the defects of some traditional catalysts currently on the market, many researchers have begun to report a large number of PET wastes converted into fine chemicals through one-pot or multi-step reactions using catalysts based on precious metals and transition metals. However, most of these methods use excessive hydrogenation to convert PET into para-xylene. The large amount of hydrogenation reaction process used is highly active and difficult to control the reaction process. The reaction environment of excess hydrogen is prone to explosions and other problems. In addition, the obtained xylene product not only has a single structure, but also xylene is a highly toxic material of the toluene class, which is very harmful to the environment and health. In addition, in order to improve the efficiency of the hydrogenation reaction, it is necessary to add a high content of precious metals or heavy metal catalysts thereof. After the reaction is completed, the precious metals and heavy metals left by the catalyst are likely to cause environmental pollution.
[0005] Therefore, a preparation method of Na+-Cu / SiO2 catalyst for PET plastic degradation is proposed. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the deficiencies in the prior art, the present invention provides a method for preparing a Na+-Cu / SiO2 catalyst for use in the degradation of PET plastics, thereby solving the above-mentioned problems.
[0008] (II) Technical solution
[0009] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation, comprising the following steps:
[0010] S1. dissolving a certain amount of copper nitrate trihydrate in a certain amount of deionized water to obtain a mixed aqueous solution;
[0011] S2, adding a certain amount of sodium chloride and a certain amount of silicon dioxide to the solution completely dissolved in S1, and mixing to obtain a suspension;
[0012] S3, stirring the suspension obtained in S2 at room temperature for 0.5 hour, and then ultrasonically treating for 0.5 hour to mix the solution uniformly;
[0013] S4, transferring the mixed solution obtained in S3 to a tetrafluoropolyvinyl chloride autoclave, and placing it in an oven at 120° C. for 3 hours;
[0014] S5, after the reaction in S4 is completed, the tetrafluoropolyvinyl chloride autoclave is cooled to room temperature, the solid product in the autoclave is filtered, and the solid product is continuously washed with deionized water until the pH value of the last filtrate is 7;
[0015] S6, placing the solid product obtained in S5 into an oven at 80° C. and drying for 12 hours, then placing the dried powdered substance into a muffle furnace and calcining it at 300° C. for 4 hours;
[0016] S7, washing the powder obtained in S6 by centrifugation, that is, dissolving the powder in appropriate amounts of dimethyl sulfoxide, ethanol, and deionized water in sequence, and then centrifuging at room temperature;
[0017] S8, filtering the solid product obtained in S7, and then drying it in an oven at 80° C. for 12 hours, and then placing the dried powdered substance in a muffle furnace and calcining it at 500° C. for 4 hours;
[0018] S9. Put the powdered product obtained in S8 into a tubular furnace and reduce it in a hydrogen atmosphere at 450° C. for 4 hours to obtain a Na + -Cu / SiO 2 catalyst.
[0019] Preferably, the amount of copper nitrate trihydrate and the amount of deionized water in S1 are accurately weighed according to the required amount and concentration of the catalyst.
[0020] Preferably, the amount of sodium chloride and silicon dioxide added in S2 is adjusted according to the desired catalyst composition.
[0021] Preferably, the heating reaction in S4 is carried out in a closed and pressure-resistant high-pressure reactor to ensure safety and reaction efficiency during the reaction.
[0022] Preferably, the calcination conditions in S6 are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1.
[0023] Preferably, the calcination conditions in S8 are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1.
[0024] Preferably, the calcination process in S6 and S8 ensures the stability and activity of the catalyst.
[0025] Preferably, the hydrogen flow rate in S9 is 150 mL·min-1, and the heating rate is 2°C·min-1.
[0026] Preferably, the hydrogen reduction process in S9 activates the copper ions in the catalyst and improves its catalytic performance.
[0027] (III) Beneficial effects
[0028] Compared with the prior art, the present invention provides a method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation, which has the following beneficial effects:
[0029] 1. This method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation is different from the traditional method for preparing Cu / SiO2 catalysts. Instead, it adopts a method combining hydrothermal and two-step annealing to prepare a catalyst that can maintain good activity and stability even under high temperature and high pressure, and improves the selectivity of the catalyst by regulating the position of Cu atoms on the carrier SiO2 by doping with alkali ions Na+. Finally, based on methanol as an alcoholysis agent, the one-pot hydrogen-free method is used. The catalyst can quantitatively convert PET into p-xylene and ethylene glycol, and these products can be easily separated from methanol by distillation, providing a new idea for the method of methanol depolymerization of discarded PET bottles.
[0030] 2. This method for preparing a Na+-Cu / SiO2 catalyst used for PET plastic degradation combines hydrothermal and two-step annealing methods to prepare a high-activity, high-stability, and high-selectivity Cu / SiO2 catalyst, and introduces an appropriate amount of NaCl during the hydration process. The proportion of Cu+ / Cu0 in the catalyst is further increased by doping with alkali ions, thereby improving the activity and selectivity of the catalyst.
[0031] 3. A method for preparing a Na+-Cu / SiO2 catalyst used for PET plastic degradation, and a method for synthesizing a modified Cu / SiO2 catalyst used in the methanol hydrolysis reaction of discarded polyethylene terephthalate (PET) bottles. Under the action of this catalyst, a low-cost method for quantitatively converting PET into p-xylene (PX) and ethylene glycol (EG) can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the connection steps of the present invention;
[0033] Figure 2 This is a transmission electron microscope image of the catalyst in Example 1 of the present invention;
[0034] Figure 3 This is a transmission electron microscope image of the catalyst in Example 2 of the present invention;
[0035] Figure 4 This is a transmission electron microscope image of the catalyst in Example 3 of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] See also Figure 1 - Figure 4 The present invention provides three technical solutions, which specifically include the following embodiments:
[0038] Embodiment 1:
[0039] A method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation comprises the following steps:
[0040] S1. Dissolve 5 parts of copper nitrate trihydrate in 50 parts of deionized water to obtain a mixed aqueous solution;
[0041] S2, adding 7 parts of sodium chloride and 25 parts of silicon dioxide to the completely dissolved solution in S1, and mixing to obtain a suspension;
[0042] S3, stirring the suspension obtained in S2 at room temperature for 0.5 hours, and then ultrasonically treating for 0.5 hours to mix the solution evenly;
[0043] S4, transferring the mixed solution obtained in S3 to a tetrafluoropolyvinyl chloride high-pressure reactor, and placing it in an oven at 120° C. for reaction for 3 hours;
[0044] S5, after the reaction in step S4 is completed, the tetrafluoropolyvinyl chloride autoclave is cooled to room temperature, the solid product in the autoclave is filtered, and the solid product is continuously washed with deionized water until the pH value of the last filtrate is 7;
[0045] S6, placing the solid product obtained in S5 into an oven at 80°C and drying for 12 hours, then placing the dried powdered substance into a muffle furnace and calcining it at 300°C for 4 hours, wherein the calcination conditions are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1;
[0046] S7, centrifugally washing the powder obtained in S6, that is, dissolving the powder in 25 parts of dimethyl sulfoxide, ethanol, and deionized water in sequence, and then centrifuging at room temperature;
[0047] S8, filtering the solid product obtained in S7, and then drying it in an oven at 80°C for 12 hours, and then placing the dried powdered substance in a muffle furnace and calcining it at 500°C for 4 hours, wherein the calcination conditions are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1;
[0048] S9. Put the powdered product obtained in S8 into a tubular furnace and reduce it in a hydrogen atmosphere at 450°C for 4 hours to obtain the catalyst, wherein the hydrogen flow rate is 150 mL·min-1 and the heating rate is 2°C·min-1.
[0049] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0050] Embodiment 2:
[0051] A method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation comprises the following steps:
[0052] S1. Dissolve 1 part of copper nitrate trihydrate in 25 parts of deionized water to obtain a mixed aqueous solution;
[0053] S2, adding 2 parts of sodium chloride and 10 parts of silicon dioxide to the solution completely dissolved in step S1, and mixing to obtain a suspension;
[0054] S3, stirring the suspension obtained in S2 at room temperature for 0.5 hours, and then ultrasonically treating for 0.5 hours to mix the solution evenly;
[0055] S4, transferring the mixed solution obtained in S3 to a tetrafluoropolyvinyl chloride high-pressure reactor, and placing it in an oven at 120° C. for reaction for 3 hours;
[0056] S5. After the reaction in S4 is completed, the tetrafluoropolyvinyl chloride autoclave is cooled to room temperature, the solid product in the autoclave is filtered, and the solid product is continuously washed with deionized water until the pH value of the last filtrate is 7;
[0057] S6, placing the solid product obtained in S5 into an oven at 80°C and drying for 12 hours, then placing the dried powdered substance into a muffle furnace and calcining it at 300°C for 4 hours, wherein the calcination conditions are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1;
[0058] S7, washing the powder obtained in S6 by centrifugation, that is, dissolving the powder in 20 parts of dimethyl sulfoxide, ethanol, and deionized water in sequence, and then centrifuging at room temperature;
[0059] S8, filtering the solid product obtained in S7, and then drying it in an oven at 80°C for 12 hours, and then placing the dried powdered substance in a muffle furnace and calcining it at 500°C for 4 hours, wherein the calcination conditions are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1;
[0060] S9. Put the powdered product obtained in S8 into a tubular furnace and reduce it in a hydrogen atmosphere at 450° C. for 4 hours to obtain the catalyst. The hydrogen flow rate is 150 mL·min-1 and the heating rate is 2° C.·min-1.
[0061] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0062] Embodiment three:
[0063] A method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation comprises the following steps:
[0064] S1. Dissolve 3 parts of copper nitrate trihydrate in 40 parts of deionized water to obtain a mixed aqueous solution;
[0065] S2, adding 4 parts of sodium chloride and 10 parts of silicon dioxide to the completely dissolved solution in S1, and mixing to obtain a suspension;
[0066] S3, stirring the suspension obtained in S2 at room temperature for 0.5 hours, and then ultrasonically treating for 0.5 hours to mix the solution evenly;
[0067] S4, transferring the mixed solution obtained in S3 to a tetrafluoropolyvinyl chloride high-pressure reactor, and placing it in an oven at 120° C. for reaction for 3 hours;
[0068] S5. After the reaction in S4 is completed, the tetrafluoropolyvinyl chloride autoclave is cooled to room temperature, the solid product in the autoclave is filtered, and the solid product is continuously washed with deionized water until the pH value of the last filtrate is 7;
[0069] S6, placing the solid product obtained in S5 into an oven at 80°C and drying for 12 hours, then placing the dried powdered substance into a muffle furnace and calcining it at 300°C for 4 hours, wherein the calcination conditions are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1;
[0070] S7, centrifugally washing the powder obtained in S6, that is, dissolving the powder in 25 parts of dimethyl sulfoxide, ethanol, and deionized water in sequence, and then centrifuging at room temperature;
[0071] S8, filtering the solid product obtained in S7, and then drying it in an oven at 80°C for 12 hours, and then placing the dried powdered substance in a muffle furnace and calcining it at 500°C for 4 hours, wherein the calcination conditions are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1;
[0072] S9. Put the powdered product obtained in S8 into a tubular furnace and reduce it in a hydrogen atmosphere at 450° C. for 4 hours to obtain the catalyst. The hydrogen flow rate is 150 mL·min-1 and the heating rate is 2° C.·min-1.
[0073] The mechanism of action of the method of the present invention is:
[0074] Compared with the preparation of traditional Cu / SiO2 catalysts, by doping Na+ to regulate the interaction between metal atoms and carriers, Na+ can act as an electron acceptor or donor to affect the charge distribution at the interface of the doped carrier. This charge transfer can change the electronic state of the carrier metal atoms, thereby improving its catalytic activity. At the same time, doping Na+ can effectively change the interface structure such as interface defects and lattice distortion between metal atoms and carriers, thereby improving the stability and catalytic activity of the carrier metal atoms. The ratio of Cu2+ / Cu0 in the catalyst is significantly increased, thereby improving the catalytic activity and selectivity of the catalyst. In addition, the catalyst is calcined by a two-step annealing method. After low-temperature calcination, the metal Na+ ions that are weakly bound to the carrier on the catalyst are removed by centrifugal washing, and then a second high-temperature calcination is performed, so that only Na atoms that are strongly bound to the Cu / SiO2 carrier are left in the catalyst, thereby increasing the stability of the catalyst under extreme reaction conditions such as high temperature and high pressure.
[0075] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation, comprising 1, characterized in that: The following steps are involved: S1. dissolving a certain amount of copper nitrate trihydrate in a certain amount of deionized water to obtain a mixed aqueous solution; S2, adding a certain amount of sodium chloride and a certain amount of silicon dioxide to the solution completely dissolved in S1, and mixing to obtain a suspension; S3, stirring the suspension obtained in S2 at room temperature for 0.5 hour, and then ultrasonically treating for 0.5 hour to mix the solution uniformly; S4, transferring the mixed solution obtained in S3 to a tetrafluoropolyvinyl chloride autoclave, and placing it in an oven at 120° C. for 3 hours; S5, after the reaction in S4 is completed, the tetrafluoropolyvinyl chloride autoclave is cooled to room temperature, the solid product in the autoclave is filtered, and the solid product is continuously washed with deionized water until the pH value of the last filtrate is 7; S6, placing the solid product obtained in S5 into an oven at 80° C. and drying for 12 hours, then placing the dried powdered substance into a muffle furnace and calcining it at 300° C. for 4 hours; S7, washing the powder obtained in S6 by centrifugation, that is, dissolving the powder in appropriate amounts of dimethyl sulfoxide, ethanol, and deionized water in sequence, and then centrifuging at room temperature; S8, filtering the solid product obtained in S7, and then drying it in an oven at 80° C. for 12 hours, and then placing the dried powdered substance in a muffle furnace and calcining it at 500° C. for 4 hours; S9. Put the powdered product obtained in S8 into a tubular furnace and reduce it in a hydrogen atmosphere at 450° C. for 4 hours to obtain a Na + -Cu / SiO 2 catalyst.
2. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The amount of copper nitrate trihydrate and the amount of deionized water in S1 are accurately weighed according to the required amount and concentration of the catalyst.
3. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The amount of sodium chloride and silicon dioxide added to S2 is adjusted according to the desired catalyst composition.
4. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The heating reaction in S4 is carried out in a closed and pressure-resistant high-pressure reactor to ensure safety and reaction efficiency during the reaction.
5. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The calcination conditions in S6 are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1.
6. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The calcination conditions in S8 are an air flow rate of 150 mL·min-1 and a heating rate of 2°C·min-1.
7. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The calcination process in S6 and S8 ensures the stability and activity of the catalyst.
8. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The hydrogen flow rate in S9 is 150 mL·min-1, and the heating rate is 2°C·min-1.
9. The method for preparing a Na+-Cu / SiO2 catalyst for PET plastic degradation according to claim 1, characterized in that: The hydrogen reduction process in S9 activates the copper ions in the catalyst and improves its catalytic performance.
Citation Information
Patent Citations
Method for preparing gasoline and anti-freezing solution from PET plastic
CN111302891A
Method for preparing aromatic hydrocarbon and ethylene glycol by depolymerizing waste polyester plastics and coupling with hydrogenolysis of ethylene carbonate
CN117088745A
KR20240040072A
Cited By
Heterogeneous catalyst for preparing p-xylene through catalytic hydrogenation of waste PET (polyethylene terephthalate) plastic as well as preparation method and application of heterogeneous catalyst
CN121314601A