Method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue

Through the modification treatment of coal gangue and microwave calcination technology, Mn-Ce/X catalyst was prepared, which solved the problems of sulfur poisoning of coal gangue catalysts and high temperature and high toxicity of traditional catalysts, and achieved efficient NO conversion rate and low temperature activity. , widens the catalytic temperature range.

CN118988385APending Publication Date: 2024-11-22INNER MONGOLIA UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411192454.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the catalyst used in NH3-SCR reaction of coal gangue is prone to sulfur poisoning due to the presence of sulfur, resulting in blockage or coverage of the active center, reducing catalytic performance, and the operating temperature of traditional V2O5-WO3 (MoO3)/TiO2 catalysts High and biotoxic, with a risk of secondary pollution.

Method used

By modifying the coal gangue, the Mn-Ce/X catalyst was prepared, and the mixture of rare earth modified coal gangue, mesoporous template agent and sodium hydroxide was used, and combined with microwave calcination technology, the cerium-manganese composite compound was formed to support X On the zeolite molecular sieve, an Mn-Ce/X catalyst with excellent performance is formed.

Benefits of technology

The NO conversion rate is significantly improved within the temperature range of 250-450°C, combining the low-temperature activity of cerium manganese catalyst with the high specific surface area of ​​coal gangue, achieving efficient removal of nitrogen oxides, and microwave calcination improves the activity and energy of the catalyst Utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988385A_ABST
    Figure CN118988385A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a Mn-Ce / X catalyst, and belongs to the field of flue gas denitration, and the method comprises the following steps: modifying coal gangue to prepare an X-type molecular sieve; and then loading the Mn-Ce oxide on the coal gangue by adopting an impregnation method, and carrying out microwave calcination to prepare the Mn-Ce / X catalyst. The catalyst provided by the invention can effectively remove nitrogen oxides, shows a relatively high NOx conversion rate in a temperature range of 250-450 DEG C, and is suitable for most working environments. According to the method, microwave heating is adopted, material calcination is more uniform through internal heating, the activity of the catalyst is improved, the X-type zeolite molecular sieve prepared from coal gangue is introduced into the Mn-Ce catalyst, the energy utilization rate is improved, and the Mn-Ce / X catalyst with excellent performance is successfully prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of flue gas denitration, and in particular to a method for preparing a Mn-Ce / X catalyst from coal gangue for NH3-SCR reaction. Background Art

[0002] Gangue is one of the largest industrial wastes in coal mining. The accumulation of large amounts of waste will lead to the occupation of land resources, soil pollution by heavy metals, and groundwater pollution. The main oxides in gangue usually include silicon dioxide, aluminum oxide, iron trioxide, calcium oxide, magnesium oxide, sodium oxide, potassium oxide, etc., of which the content of silicon dioxide and aluminum oxide exceeds 65%, and it also contains other trace elements. Unprocessed gangue particles are large and uneven in size, and the direct utilization performance is not ideal. Therefore, it is usually modified in the chemical industry for the preparation of zeolites, molecular sieve catalysts, etc.

[0003] For the catalyst used in NH3-SCR reaction, a larger specific surface area, pore volume and average pore size are conducive to the adsorption of NO and NH3. Coal gangue contains a small amount of SO3 compounds. The presence of sulfur will cause sulfur poisoning of the catalyst. SO3 reacts with NH3 to generate ammonium sulfate and ammonium bisulfate, and reacts with manganese oxide through a series of reactions to generate byproducts such as manganese sulfate. These substances are difficult to decompose, block or cover the active center, reduce the specific surface area, and cause the catalyst to be temporarily or even permanently deactivated. Therefore, the coal gangue must be crushed, screened and roasted first. The coal gangue is easier to modify after roasting.

[0004] Although the traditional V2O5-WO3(MoO3) / TiO2 catalyst has good catalytic performance in the temperature range of 200-250℃, it has many disadvantages, such as high operating temperature, biological toxicity of the active component V2O5, and easy secondary pollution. The preparation of Mn-Ce / X catalyst by rare earth modified coal gangue is a new type of catalytic material, in which the cerium-manganese composite compound is evenly distributed on the surface of coal gangue, thereby meeting the application requirements during use and expanding the scope of application. Therefore, this new material has great application prospects.

[0005] Some international institutions have carried out research in this area, but there are no reports on how to use coal gangue to prepare Mn-Ce / X catalytic materials. Summary of the invention

[0006] The problem to be solved by the present invention is to provide a method for preparing Mn-Ce / X catalyst material from coal gangue.

[0007] The technical solution of the present invention:

[0008] A method for preparing a Mn-Ce / X catalyst by using rare earth modified coal gangue, the method comprising the following steps:

[0009] (1) Grinding coal gangue, removing carbon and desulfurizing at high temperature, mixing the burned coal gangue with anhydrous sodium carbonate and alkali melting to obtain a blue-green solid, then mixing and stirring with a sodium hydroxide solution according to a certain solid-liquid ratio, adding a certain amount of a mesoporous template agent, stirring, crystallizing, washing, and drying, and heating in a muffle furnace to obtain an X-type zeolite molecular sieve catalyst;

[0010] (2) The Mn-Ce compound is loaded on the X-type zeolite molecular sieve catalyst in a mass ratio of 1 to 5:20, and finally calcined by microwave to obtain a Mn-Ce / X catalyst.

[0011] Preferably, the mass ratio of the coal gangue, anhydrous sodium carbonate and mesoporous template is 2:4:1; the concentration of the sodium hydroxide solution used is 3 mol / L, and the solid-liquid ratio of the blue-green solid to sodium hydroxide is 0.1 g / mL.

[0012] Preferably, the heating rate of the muffle furnace is: heating to 500° C. at a heating rate of 1° C. / min.

[0013] Preferably, the concentration of the NaOH solution is 3 mol / L.

[0014] Preferably, the molar ratio of Mn to Ce in the Mn-Ce mixed oxide is 2 to 3:1, and the manganese source and cerium source are respectively manganese nitrate and cerium nitrate hexahydrate.

[0015] Preferably, the mesoporous template agent is hexadecyltrimethylammonium bromide.

[0016] Preferably, the microwave frequency is 2.45 GHz.

[0017] Beneficial effects of the present invention:

[0018] 1. The present invention prepares an X-type molecular sieve by modifying coal gangue; then uses an impregnation method to load Mn-Ce oxide on the coal gangue, and then prepares a Mn-Ce / X catalyst with excellent performance by microwave calcination.

[0019] 2. The present invention combines the good low-temperature activity of the cerium manganese catalyst with the high specific surface area of ​​coal gangue to effectively remove nitrogen oxides. The prepared catalyst exhibits a high NO conversion rate in the temperature range of 250 to 450°C and can be applied to most working environments.

[0020] 3. The present invention adopts microwave heating to make the material calcined more uniformly through internal heating, thereby improving the activity of the catalyst. The X-type zeolite molecular sieve prepared from coal gangue is introduced into the Mn-Ce catalyst, thereby improving the energy utilization rate, and successfully preparing a Mn-Ce / X catalyst with excellent performance. The Mn-Ce / X catalyst of the present invention provides a new way for low-temperature reduction of NO. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A comparison chart of NOx conversion rates of the catalysts provided in Examples 1-5 of the present invention; Specific implementation methods

[0023] The specific implementation modes of the present invention are described in detail below through examples.

[0024] Example 1

[0025] A method for preparing a Mn-Ce / X catalyst by using rare earth modified coal gangue comprises the following steps:

[0026] (1) Grind 10 g of coal gangue, pass it through a 100-mesh sieve, and then roast it in a muffle furnace at 850° C. for 4 h to perform high-temperature carbon removal and desulfurization. Mix the roasted coal gangue with 20 g of anhydrous sodium carbonate and roast it at 850° C. for 3 h to obtain a blue-green solid;

[0027] The obtained blue-green solid was mixed with 3 mol / L sodium hydroxide solution with a solid-liquid ratio of 0.1 g / mL, and 5 g of hexadecyltrimethylammonium bromide was added. The mixture was stirred at room temperature for 12 hours, and then transferred to a reactor and crystallized at 100°C for 24 hours. The reaction product was washed three times with deionized water and ethanol, and then dried at 100°C for 10 hours, and heated at 500°C in a muffle furnace for 3 hours to obtain an X-type zeolite molecular sieve.

[0028] (2) Manganese nitrate and cerium nitrate hexahydrate were loaded on X-type zeolite molecular sieve by impregnation method to prepare Mn-Ce / X catalyst.

[0029] 0.052 g of manganese nitrate and 0.05 g of cerium nitrate hexahydrate (the molar ratio of Mn / Ce is 2.5:1) were weighed, 50 ml of deionized water was added after mixing, and ultrasonic dispersion was performed for 30 minutes to obtain a precursor solution; 2 g of X-type zeolite molecular sieve was added to the precursor solution, the mixture was ultrasonically dispersed for 15 minutes, transferred to an 80°C oil bath, stirred and heated for 3 hours, and then the heated sample was taken out and dried at 80°C for 12 hours; finally, it was calcined at 500°C for 3 hours by microwave to obtain a Mn-Ce / X catalyst.

[0030] The heating rate during microwave heating was 10°C / min and the microwave frequency was 2.45 GHz.

[0031] Example 2

[0032] A method for preparing a Mn-Ce / X catalyst by using rare earth modified coal gangue comprises the following steps:

[0033] (1) Grind 10 g of coal gangue, pass through a 100-mesh sieve, and roast in a muffle furnace at 850° C. for 4 h to perform high-temperature carbon removal and desulfurization. Mix the roasted coal gangue with 20 g of anhydrous sodium carbonate and roast at 850° C. for 3 h to obtain a blue-green solid;

[0034] The obtained blue-green solid was mixed with 3 mol / L sodium hydroxide solution and stirred to a solid-liquid ratio of 0.1 g / mL, and then 5 g of mesoporous template agent hexadecyltrimethylammonium bromide was added, stirred at room temperature for 12 hours, transferred to a reactor, and crystallized at 100°C for 24 hours. The obtained material was washed three times with deionized water and ethanol, then dried at 100°C for 10 hours, and then heated at 500°C in a muffle furnace for 3 hours to obtain an X-type zeolite molecular sieve.

[0035] (2) 0.104 g of manganese nitrate and 0.1 g of cerium nitrate hexahydrate were added to 50 ml of deionized water (the molar ratio of Mn / Ce was about 2.5:1), followed by ultrasonic dispersion for 30 min to obtain a mixed precursor solution, and then 2 g of X-type zeolite molecular sieve was added to the precursor solution, and the mixture was ultrasonically dispersed for 15 min, and then transferred to an 80°C oil bath and stirred and heated for 3 hours, and then the heated sample was dried at 80°C for 12 hours. Finally, it was calcined at 500°C for 3 hours by microwave to obtain a Mn-Ce / X catalyst.

[0036] Example 3

[0037] A method for preparing a Mn-Ce / X catalyst by using rare earth modified coal gangue comprises the following steps:

[0038] (1) 10 g of coal gangue was ground, passed through a 100-mesh sieve, and calcined in a muffle furnace at 850° C. for 4 h to perform high-temperature carbon removal and desulfurization. The burned coal gangue was mixed with 20 g of anhydrous sodium carbonate and calcined at 850° C. for 3 h to obtain a blue-green solid. The obtained blue-green solid was mixed and stirred with a 3 mol / L sodium hydroxide solution at a solid-liquid ratio of 0.1 g / mL, and 5 g of a mesoporous template agent, hexadecyltrimethylammonium bromide, was added, stirred at room temperature for 12 h, transferred to a reactor, and crystallized at 100° C. for 24 h. The reaction product was washed three times with deionized water and ethanol, and then dried at 100° C. for 10 h, and then heated in a muffle furnace at 500° C. for 3 h to obtain an X-type zeolite molecular sieve.

[0039] (2) 0.156 g of manganese nitrate and 0.15 g of cerium nitrate hexahydrate were mixed and added into 50 ml of deionized water, with a molar ratio of Mn / Ce of about 2.5:1, followed by ultrasonic dispersion for 30 minutes to obtain a mixed precursor solution, and then 2 g of X-type zeolite molecular sieve was added to the precursor solution, and the mixture was ultrasonically dispersed for 15 minutes, and then transferred to an 80°C oil bath and stirred and heated for 3 hours, and then the heated sample was dried at 80°C for 12 hours; finally, it was calcined at 500°C for 3 hours by microwave heating to obtain a Mn-Ce / X catalyst.

[0040] Example 4

[0041] A method for preparing a Mn-Ce / X catalyst by using rare earth modified coal gangue comprises the following steps:

[0042] (1) 10 g of coal gangue was ground, passed through a 100-mesh sieve, and calcined in a muffle furnace at 850° C. for 4 h to perform high-temperature carbon removal and desulfurization. The burned coal gangue was mixed with 20 g of anhydrous sodium carbonate and calcined at 850° C. for 3 h to obtain a blue-green solid. The obtained blue-green solid was then mixed and stirred with a 3 mol / L sodium hydroxide solution at a solid-to-liquid ratio of 0.1 g / mL. 5 g of a mesoporous template agent, hexadecyltrimethylammonium bromide, was added, stirred at room temperature for 12 h, transferred to a reactor, and crystallized at 100° C. for 24 h. The reaction product was washed three times with deionized water and ethanol, then dried at 100° C. for 10 h, and then heated in a muffle furnace at 500° C. for 3 h to obtain an X-type zeolite molecular sieve.

[0043] (2) 0.208 g of manganese nitrate and 0.2 g of cerium nitrate hexahydrate were added to 50 ml of deionized water, with a molar ratio of Mn / Ce of about 2.5:1, and ultrasonically dispersed for 30 minutes to obtain a mixed precursor solution. Then, 2 g of X-type zeolite molecular sieve was added to the precursor solution, and the mixture was ultrasonically dispersed for 15 minutes. Then, it was transferred to an 80°C oil bath and stirred and heated for 3 hours, and then the heated sample was dried at 80°C for 12 hours. Finally, it was calcined at 500°C for 3 hours by microwave to obtain a Mn-Ce / X catalyst.

[0044] Comparative Example 5

[0045] A method for producing an X-type zeolite molecular sieve catalyst comprises the following steps:

[0046] 10g of coal gangue was ground, passed through a 100-mesh sieve, and calcined at 850°C for 4h in a muffle furnace for high-temperature carbon removal and desulfurization. The calcined coal gangue was mixed with 20g of anhydrous sodium carbonate and calcined at 850°C for 3h to obtain a blue-green solid. The obtained blue-green solid was mixed and stirred with a 3mol / L sodium hydroxide solution with a solid-liquid ratio of 0.1g / mL, and 5g of hexadecyltrimethylammonium bromide was added. The mixture was stirred at room temperature for 12 hours, transferred to a reactor, and crystallized at 100°C for 24 hours. The reaction product was washed three times with deionized water and ethanol, and then dried at 100°C for 10 hours, and then heated at 500°C in a muffle furnace for 3 hours to obtain an X-type zeolite molecular sieve catalyst.

[0047] The catalysts obtained in the above examples and comparative examples were tested, and the specific tests were as follows:

[0048] In order to simulate the industrial flue gas emission environment in actual applications, the denitrification activity data of the catalyst are evaluated by the NH3-SCR activity test device, which consists of a gas distribution system, a temperature control system, and an exhaust gas analysis system. 0.2g of each of the above-prepared catalysts is taken and placed on the quartz wool of the reaction tube. A mixed gas of NO, O2, NH3, and N2 is passed into the reaction tube. The initial concentrations of NH3 and NO in the mixed gas are both 500ppm, the O2 content is 6vol.%, and N2 is used to balance with other gases. The temperature in the reaction tube is 100℃~500℃.

[0049] NO x The concentration was measured by a flue gas analyzer (Laoying 3002). The temperature was raised from 100°C at a heating rate of 10°C / min, and a temperature observation point was set every 50°C until the temperature reached 500°C. The NO concentration in the reactor inlet and outlet gas was recorded. x NO concentration can be obtained by calculation x conversion rate.

[0050] Depend on Figure 1 It can be seen that at different temperatures, when the Mn-Ce / X catalyst is used in the test device, NO x The conversion rates are higher than those using the X-type zeolite molecular sieve catalyst, indicating that the catalytic activity of the Mn-Ce / X catalyst of the present invention is significantly higher than that of the X-type zeolite molecular sieve catalyst.

[0051] Figure 1 It can also be seen that the catalyst of Example 3 has NO x The conversion rate is above 80%. This indicates that the doping of cerium and manganese in the catalyst of the present invention improves the catalytic activity to a certain extent and broadens the catalytic temperature range, but when the doping amount of cerium and manganese is too high, the catalytic activity decreases.

Claims

1. A method for preparing a Mn-Ce / X catalyst by using rare earth modified coal gangue, characterized in that: The method comprises the following steps: (1) Grinding coal gangue, removing carbon and desulfurizing at high temperature, mixing the burned coal gangue with anhydrous sodium carbonate and alkali melting to obtain a blue-green solid, then mixing and stirring with a sodium hydroxide solution according to a certain solid-liquid ratio, adding a certain amount of a mesoporous template agent, stirring, crystallizing, washing, and drying, and heating in a muffle furnace to obtain an X-type zeolite molecular sieve catalyst; (2) The Mn-Ce compound is loaded on the X-type zeolite molecular sieve catalyst in a mass ratio of 1 to 5:20, and finally calcined by microwave to obtain a Mn-Ce / X catalyst.

2. The method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue according to claim 1, characterized in that: The mass ratio of coal gangue, anhydrous sodium carbonate and mesoporous template is 2:4:1; the concentration of sodium hydroxide solution used is 3 mol / L, and the solid-liquid ratio of blue-green solid to sodium hydroxide is 0.1 g / mL.

3. The method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue according to claim 1, characterized in that: The heating rate of the muffle furnace is: heating to 500° C. at a heating rate of 1° C. / min.

4. The method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue according to claim 1, characterized in that: The concentration of the NaOH solution is 3 mol / L.

5. The method for preparing the rare earth modified coal gangue Mn-Ce / X catalyst according to claim 1, characterized in that: The molar ratio of Mn to Ce in the Mn-Ce mixed oxide is 2-3:1, and the manganese source and the cerium source are respectively manganese nitrate and cerium nitrate hexahydrate.

6. The method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue according to claim 1, characterized in that: The mesoporous template agent is hexadecyltrimethylammonium bromide.

7. The method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue according to claim 1, characterized in that: The microwave frequency is 300 MHz to 10 GHz.

8. The method for preparing Mn-Ce / X catalyst from rare earth modified coal gangue according to claim 7, characterized in that: The microwave frequency is 2.45 GHz.

Citation Information

Patent Citations

  • Preparation method and application of X-type zeolite molecular sieve catalyst

    CN112958144A

  • Low-temperature adsorption catalyst and preparation method thereof

    CN116273150A

  • Sludge carrier activated rare earth-based denitration catalyst as well as preparation method and application thereof

    CN117654537A

  • Molecular sieve and its preparation method

    US20210283586A1