Production process of carbon steel grade in continuous casting and rolling of wire rod
By conducting component analysis and proportioning of steel materials, combined with pretreatment and protective casting technology of arc furnaces and refining furnaces, the process of cooling and heating of medium carbon steel billets is cancelled, and the direct delivery and rolling of medium carbon steel continuous casting hot billets is realized. , solves the high production cost problem caused by the chaotic use of steel materials in traditional processes, and reduces the difficulty and cost of dephosphorization and desulfurization operations.
Patent Information
- Application Number
- CN202411222151.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-22
AI Technical Summary
The chaotic use of steel materials in the traditional carbon steel production process leads to high phosphorus and sulfur content and large fluctuations in primary molten steel, which increases production costs and refining agent consumption, and the high steel output temperature causes peroxidation of the molten steel, reducing the yield of steel material .
By conducting composition analysis and proportioning of steel materials, pretreatment using 50%-80% stamping thin plate crushed material, 5%-10% pig iron and 10%-30% scrap steel ratios, electric arc furnace and refining furnace for pre-treatment using Deoxidation of slag, protective casting is carried out using large-pack long water outlets and SEN water outlets to protect the protective casting. The process of cooling and heating of medium carbon steel billets is abolished to realize direct delivery and rolling of medium carbon steel continuous casting hot billets, and the auxiliary of electromagnetic induction billet heater is added. heating.
Effectively reduce the difficulty and cost of dephosphorization and desulfurization operations, improve the quality of steel billets, reduce the consumption of dephosphorization and desulfurization materials, realize the direct delivery and direct rolling production process of medium-carbon steel continuous casting hot billets, and reduce the management of steel billets and Site occupation reduces production costs.
Smart Images

Figure CN118988973A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steelmaking, and in particular to a production process for medium-carbon steel grades through continuous casting and rolling of wire rods. Background Art
[0002] At present, all iron and steel metallurgical enterprises are equipped with continuous casting production lines. Continuous casting of steel is an essential part of modern iron and steel metallurgical technology, and the continuous casting ratio represents the advanced level of iron and steel metallurgical technology. Continuous casting machines are used to produce round billets, square billets, slabs and other billets for rolling mills. At present, the domestic production of medium-carbon steel mainly adopts the traditional smelting-cooling-reheating-rolling production process. The traditional production process of medium-carbon steel wire is divided into two parts. The steelmaking process is: steel material → electric arc furnace → refining furnace → continuous casting → fixed length → billet cooling, and the rolling process is: billet heating → rough rolling → medium rolling → finishing rolling → water cooling → wire laying → air cooling → coiling → inspection → packaging → weighing and hanging → unloading → storage.
[0003] At present, in the traditional process, steel materials are used chaotically, the initial phosphorus and sulfur contents of the primary molten steel in the electric arc furnace are high and fluctuate greatly, which increases the production cost. The high steelmaking temperature causes overoxidation of the primary molten steel, reduces the steel material recovery rate, and increases the consumption of silicon carbide, a deoxidizer in the refining furnace, which is not conducive to clean steel production and increases production costs. Summary of the invention
[0004] The purpose of the present invention is to provide a process for producing medium carbon steel by continuous casting and rolling of wire rod, aiming to solve the problem of high production cost of existing carbon steel production processes.
[0005] To achieve the above object, the present invention provides a process for producing medium carbon steel by continuous casting and rolling of wire rod, comprising the following steps:
[0006] Proportioning of steel materials to be processed;
[0007] The proportioned steel material is placed in an electric arc furnace for pretreatment to obtain primary molten steel;
[0008] Putting the primary molten steel into a refining furnace for treatment to obtain molten steel;
[0009] The molten steel is protected and casted by using a ladle long nozzle and a SEN nozzle protection to obtain a steel billet;
[0010] Sizing the steel billet;
[0011] Rolling the steel billet after the length is set;
[0012] water cooling the steel billet after the pressing process;
[0013] The cooled steel billet is subjected to a wire-spinning process to obtain a wire rod.
[0014] Among them, in "proportioning of steel materials to be processed", it includes:
[0015] Conduct composition analysis on various steel materials to obtain composition data;
[0016] The steel is proportioned based on the composition data.
[0017] Among them, in "proportioning steel based on the composition data", the proportion of steel is 50%-80% stamping sheet scraps + 5%-10% pig iron + 10%-30% scrap steel.
[0018] Among them, in "putting the primary molten steel into a refining furnace for treatment to obtain molten steel", the treatment includes using silicon carbide to deoxidize the slag and make white slag, the white slag duration is ≥20 minutes, and the sulfur content is controlled to be ≤0.015%. After the deoxidation, desulfurization, carbon addition and alloying operations of the deoxidizing material are completed, the molten steel is calcium treated, the soft blowing time is 8-20 minutes, and the double bottom blowing of argon is 20-60L / min.
[0019] Among them, in "protectively casting the molten steel through a large ladle long nozzle and a SEN nozzle protection to obtain a steel billet", the pouring superheat is 20-45°C, the pulling speed is 3.2-4.0m / min, the secondary cooling water full water cooling water ratio is 0.7-1.2L / kg, and the billet shell thickness is 40-60mm.
[0020] Among them, in "rolling the steel billet after sizing", the rolling treatment includes rough rolling, intermediate rolling and finish rolling. The processing temperature of the rough rolling is 760℃-1000℃, and the tail cutting length is ≤150mm. The thickness of the intermediate billet of the intermediate rolling is 20mm-80mm, the head cutting length is ≤350mm, and the tail cutting length is ≤450mm. The processing temperature of the finish rolling is 900℃-1000℃, and the tail cutting length is ≤800mm.
[0021] Among them, in "the steel billet after cooling is subjected to wire-spinning treatment to obtain wire rod.", the wire-spinning temperature is 850-1000°C.
[0022] The invention discloses a production process of medium-carbon steel grades in continuous casting and rolling of wire rod, comprising the following steps: proportioning steel materials to be processed; placing the proportioned steel materials into an electric arc furnace for pretreatment to obtain primary molten steel; placing the primary molten steel into a refining furnace for treatment to obtain molten steel; protectively casting the molten steel through a large ladle long nozzle and a SEN nozzle protection to obtain a steel billet; sizing the steel billet; rolling the sizing steel billet; water cooling the steel billet after the pressing treatment; spinning the steel billet after the cooling treatment to obtain wire rod. The invention fully utilizes the waste heat of the continuously cast steel billet, eliminates the process link of first cooling and then heating the medium-carbon steel billet, and realizes the production process of directly sending and rolling the continuously cast hot billet of medium-carbon steel grades. The invention fully utilizes the waste heat of the continuously cast steel billet, eliminates the process link of first cooling and then heating the medium-carbon steel billet, and realizes the production process of directly sending and rolling the continuously cast hot billet of medium-carbon steel grades. Control the reasonable proportion of various steel materials, effectively solve the problem of high and fluctuating initial phosphorus and sulfur content in molten steel caused by chaotic use of steel materials in electric furnace steelmaking to produce medium-carbon steel, reduce the difficulty of dephosphorization and desulfurization operations, and reduce the consumption of lime for dephosphorization and desulfurization materials. Realize the production process of direct delivery and direct rolling of hot billets for continuous casting of medium-carbon steel, cancel the original auxiliary processes such as billet length collection and secondary heating in the heating furnace, reduce the loss of head and tail per ton of steel and the operating cost of auxiliary processes. Considering that a certain amount of cold billets will be generated during the start and stop of continuous casting and due to failure of the rolling mill, an electromagnetic induction billet heater is added as an auxiliary heating equipment. In normal production, the cold billets are heated by the electromagnetic induction billet heater and then returned to the rolling team to avoid mixing steel and site occupation caused by billet management, thereby solving the problem of high production cost of the existing carbon steel production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 The present invention provides a flow chart of a process for producing medium-carbon steel by continuous casting and rolling of wire rods.
[0025] Figure 2 It is a flow chart for proportioning the steel materials to be processed. DETAILED DESCRIPTION
[0026] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0027] See also Figure 1 to Figure 2 The present invention provides a process for producing medium carbon steel by continuous casting and rolling of wire rod, comprising the following steps:
[0028] S1 proportions the steel materials to be processed;
[0029] S11 performs composition analysis on various steel materials to obtain composition data;
[0030] Specifically, through component testing of various types of steel materials, it was found that the pressed plate fragments (industrial scrap steel) were low-sulfur and low-phosphorus steel with a sulfur content of about 0.008% and a phosphorus content of about 0.020%. However, the pile was relatively small, which affected the material feeding. It was found that the composition of social scrap steel was complex, with high phosphorus and sulfur contents and large fluctuations. Among them, the sulfur content of a certain material was detected to be about 0.28%, and the phosphorus content was about 0.056%. It was judged to be free-cutting steel, and the social scrap steel (scrap steel) pile was relatively large.
[0031] S12 mixes the steel based on the composition data.
[0032] The steel ratio is 50%-80% stamping sheet scraps + 5%-10% pig iron + 10%-30% scrap steel.
[0033] Specifically, the steel material ratio is: 50%-80% stamping sheet scraps + 5%-10% pig iron + 10%-30% social scrap steel. The initial phosphorus content of the molten steel is controlled at 0.025%-0.040%, and the initial sulfur content of the molten steel is controlled at 0.015%-0.040%.
[0034] S2 puts the proportioned steel material into an electric arc furnace for pretreatment to obtain primary molten steel;
[0035] Specifically, the steel material is evenly added to the electric arc furnace, the foam slag is controlled throughout the process, the oxygen lance + bottom blowing is combined, the furnace door oxygen lance and the furnace wall oxygen lance are used together, and the bottom blowing air-permeable brick is used to increase the stirring power of the molten steel. The end point of the electric arc furnace steel tapping is controlled: the carbon content of the steel tapping is controlled at 0.12%-0.40%, the phosphorus content is ≤0.020%, and the steel tapping temperature is 1580-1620℃. The end point oxygen content is 300-700ppm. Lime, fluorite, alloy, and silicon carbide are added during the steel tapping process.
[0036] S3: placing the primary molten steel into a refining furnace for treatment to obtain molten steel;
[0037] The treatment includes using silicon carbide to deoxidize slag and make white slag, the white slag duration is ≥20 minutes, the sulfur content is controlled to be ≤0.015%, and after the deoxidation, desulfurization, carbon addition and alloying operations of the deoxidizing material are completed, the molten steel is treated with calcium, the soft blowing time is 8-20 minutes, and the double bottom blowing of argon is 20-60L / min.
[0038] Specifically, the refining furnace uses silicon carbide for slag deoxidation and white slag production. The duration of white slag is ≥20 minutes, the sulfur content is controlled to be ≤0.015%, the initial sulfur content is low, the desulfurization difficulty is small, and the lime consumption is 6-10kg / t. The oxygen activity of steel is low. After the deoxidation, desulfurization, carbonization and alloying operations of the deoxidized material are completed, the molten steel is treated with calcium, the soft blowing time is 8-20min, and the double bottom blowing of argon is 20-60L / min.
[0039] S4 performs protective casting on the molten steel through a large ladle long nozzle and a SEN nozzle protection to obtain a steel billet;
[0040] The pouring superheat is 20-45°C, the pulling speed is 3.2-4.0m / min, the secondary cooling water full water cooling water ratio is 0.7-1.2L / kg, and the shell thickness is 40-60mm.
[0041] Specifically, continuous casting uses a large ladle long nozzle, SEN nozzle protection casting, electromagnetic stirring, and by adjusting the superheat of 20-45℃, the pulling speed of 3.2-4.0m / min, the secondary cooling water full water cooling water volume of 0.7-1.2L / kg, the billet with liquid core straightening, and the billet shell thickness of 40-60mm, the surface temperature of the continuous casting billet during shearing is controlled to reach 950-1200℃, and the core temperature reaches 1100-1300℃ without internal defects. To meet the rolling needs.
[0042] S5 sizes the steel billet;
[0043] Specifically, the steel billets do not need to be transported by vehicles, and do not need to enter a heating furnace to heat up the steel billets. The fixed length is only limited by the total length of the shearing machine roller, cooling bed, and direct feed roller, which can be adjusted within 50m. The temperature difference between the head and tail of the steel billet needs to be controlled. The steel billets come out of the cooling bed and directly enter the No. 1 rolling mill through the long roller for rolling.
[0044] S6 performs rolling processing on the steel billet after being cut to size;
[0045] The rolling process includes rough rolling, intermediate rolling and finishing rolling. The processing temperature of the rough rolling is 760°C-1000°C, and the tail cutting length is ≤150mm. The thickness of the intermediate billet of the intermediate rolling is 20mm-80mm, the head cutting length is ≤350mm, and the tail cutting length is ≤450mm. The processing temperature of the finishing rolling is 900°C-1000°C, and the tail cutting length is ≤800mm.
[0046] Specifically, rough rolling. 760-1000℃. The head and tail are cut at the No. 1 flying shear, and the cutting length is ≤150mm. The rolling temperature is monitored in real time, and when the head temperature is too low, it is fed back to the continuous casting process to adjust the water ratio of the secondary cooling water. In the intermediate rolling, the thickness of the intermediate billet is controlled at 20-80mm. The head and tail are cut at the No. 2 flying shear, and the head cutting length is ≤350mm, and the tail cutting length is ≤450mm. In the finishing rolling, the temperature before finishing rolling is controlled at 900-1000℃. The head and tail are cut at the No. 3 flying shear, and the cutting length is ≤800mm.
[0047] S7 water-cools the steel billet after the pressing process;
[0048] Specifically, when the head of the coil is penetrated by water, the tail is penetrated by water, and the water tank is fully opened to reduce the temperature difference between the head and the tail, and control the difference in tensile strength between the head and the tail within 50MPa.
[0049] S8 performs a wire spinning process on the steel billet after cooling to obtain a wire rod.
[0050] The spinning temperature is 850-1000°C.
[0051] Specifically, the spinning temperature is controlled at 850-1000°C. Air cooling, coiling, inspection, packaging, weighing and labeling, coil unloading and storage can be carried out normally.
[0052] Embodiment 1
[0053] Proportion and smelting: Steel material ratio: 60% stamping sheet scraps + 8% pig iron + 32% social scrap steel.
[0054] Arc furnace operation: uniform charging, full foam slag control, oxygen lance + bottom blowing composite blowing to ensure sufficient stirring of molten steel. When tapping, the carbon content is controlled at 0.25%, the phosphorus content is ≤0.018%, and the tapping temperature is 1600℃.
[0055] Refining and continuous casting: The refining furnace uses silicon carbide for slag deoxidation, and the white slag lasts for 25 minutes to ensure that the sulfur content is ≤0.012%. During the continuous casting process, the superheat is maintained at 30°C, the casting speed is 3.6m / min, and the secondary cooling water is fully cooled with a specific water volume of 0.9L / kg to ensure the quality of the steel billet.
[0056] Subsequent process: The cut length is set to 45m, and the temperature difference between the head and the tail is reduced to the minimum. The rough rolling temperature is 900℃, the intermediate rolling intermediate billet thickness is controlled at 50mm, and the finishing rolling steel feeding temperature is 950℃. The water cooling link ensures a small temperature difference between the head and the tail, and the difference in tensile strength is controlled within 40MPa. The wire laying temperature is controlled at 925℃.
[0057] Embodiment 2
[0058] Proportion and smelting: Steel material ratio: 70% stamping sheet scraps + 7% pig iron + 23% social scrap steel.
[0059] The operation of the electric arc furnace is strengthened by the use of bottom blowing air bricks to improve the stirring efficiency. The carbon content of the steel is 0.30%, the phosphorus content is ≤0.015%, and the steel temperature is 1590℃.
[0060] Refining and continuous casting: The duration of white slag in the refining furnace is extended to 22 minutes, and the sulfur content is more strictly controlled to ≤0.010%. The continuous casting superheat is set at 35°C and the casting speed is 3.8m / min to ensure that the billet has no internal defects.
[0061] Subsequent process: The fixed length is 48m, and the temperature difference between the head and tail of the billet is further reduced. The rough rolling, intermediate rolling and finishing rolling temperatures are set at 950℃, 800℃ and 980℃ respectively to ensure the rolling effect. The difference in tensile strength after water cooling is controlled within 35MPa. The wire laying temperature is set at 900℃.
[0062] Table 1: Comparison of initial sulfur content in molten steel
[0063]
[0064] Table 2: Comparison of carbon content of steel produced by electric furnace smelting of all scrap steel
[0065] Carbon content of steel produced by traditional process % Carbon content of steel produced by new process % 0.06 0.16 0.05 0.20 0.04 0.14 0.06 0.13 0.06 0.12 0.04 0.14
[0066] Table 3 Comparison of natural gas consumption
[0067]
[0068]
[0069] Through the development of continuous casting and direct rolling of medium carbon steel production technology, the problems of difficult desulfurization and dephosphorization operation, large lime consumption and high cost caused by traditional processes can be effectively solved. The problem of high steel temperature in the electric arc furnace causing overoxidation of molten steel and reduced steel yield can be solved. The problem of high input costs of fuel, labor, equipment, etc. caused by secondary heating of steel billets can be solved, which is conducive to the smooth progress of continuous casting and higher production efficiency.
[0070] Beneficial effects:
[0071] 1. Make full use of the waste heat of the continuous casting billet, cancel the process of cooling the medium carbon steel billet first and then heating it, and realize the direct delivery and direct rolling production process of continuous casting hot billet of medium carbon steel grades.
[0072] 2. Control the reasonable proportion of various steel materials, effectively solve the problem of high and fluctuating initial phosphorus and sulfur content in molten steel caused by chaotic use of steel materials in electric furnace steelmaking to produce medium-carbon steel, reduce the difficulty of dephosphorization and desulfurization operations, and reduce the consumption of lime for dephosphorization and desulfurization materials.
[0073] 3. Realize the production process of direct delivery and direct rolling of hot continuous casting billets for medium-carbon steel grades, cancel the original auxiliary processes such as billet collection and secondary heating in the heating furnace, reduce the loss of head and tail per ton of steel and the operating cost of auxiliary processes.
[0074] 4. Considering that a certain amount of cold billets will be generated when continuous casting starts or stops pouring, or due to failure of the rolling mill, an electromagnetic induction billet heater is added as an auxiliary heating equipment. In normal production, the cold billets are heated by the electromagnetic induction billet heater and then returned to the rolling team to avoid mixing of steel and site occupation caused by billet management.
[0075] The above disclosure is only a preferred embodiment of the production process of medium-carbon steel grades of wire continuous casting and rolling of the present invention. Of course, this cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiments and equivalent changes made in accordance with the claims of the present invention still fall within the scope covered by the invention.
Claims
1. A process for producing medium carbon steel by continuous casting and rolling of wire rod, characterized in that: The following steps are involved: Proportioning of steel materials to be processed; The proportioned steel material is placed in an electric arc furnace for pretreatment to obtain primary molten steel; Putting the primary molten steel into a refining furnace for treatment to obtain molten steel; The molten steel is protected and casted by using a ladle long nozzle and a SEN nozzle protection to obtain a steel billet; Sizing the steel billet; Rolling the steel billet after the length is set; water cooling the steel billet after the pressing process; The cooled steel billet is subjected to a wire-spinning process to obtain a wire rod.
2. The process for producing medium carbon steel by continuous casting and rolling of wire rod according to claim 1, characterized in that: In "proportioning of steel materials to be processed", it includes: Conduct composition analysis on various steel materials to obtain composition data; The steel is proportioned based on the composition data.
3. The process for producing medium carbon steel by continuous casting and rolling of wire rod as claimed in claim 2, characterized in that: In "proportioning steel based on the composition data", the proportion of the steel proportion is 50%-80% stamping sheet scraps + 5%-10% pig iron + 10%-30% scrap steel.
4. The process for producing medium carbon steel by continuous casting and rolling of wire rod according to claim 1, characterized in that: In "putting the primary molten steel into a refining furnace for treatment to obtain molten steel", the treatment includes using silicon carbide to deoxidize the slag and make white slag, the white slag duration is ≥20 minutes, the sulfur content is controlled to be ≤0.015%, and after the deoxidation, desulfurization, carbon addition and alloying operations of the deoxidizing material are completed, the molten steel is calcium treated, the soft blowing time is 8-20 minutes, and the double bottom blowing of argon is 20-60L / min.
5. The process for producing medium carbon steel by continuous casting and rolling of wire rod according to claim 1, characterized in that: In "protectively casting the molten steel through a large ladle long nozzle and a SEN nozzle protection to obtain a steel billet", the pouring superheat is 20-45°C, the pulling speed is 3.2-4.0m / min, the secondary cooling water full water cooling water ratio is 0.7-1.2L / kg, and the billet shell thickness is 40-60mm.
6. The process for producing medium carbon steel by continuous casting and rolling of wire rod according to claim 1, characterized in that: In "rolling the steel billet after sizing", the rolling treatment includes rough rolling, intermediate rolling and finish rolling. The treatment temperature of the rough rolling is 760°C-1000°C, and the tail cutting length is ≤150mm. The thickness of the intermediate billet of the intermediate rolling is 20mm-80mm, the head cutting length is ≤350mm, and the tail cutting length is ≤450mm. The treatment temperature of the finish rolling is 900°C-1000°C, and the tail cutting length is ≤800mm.
7. The process for producing medium carbon steel by continuous casting and rolling of wire rod according to claim 1, characterized in that: In "the steel billet after cooling is subjected to a wire-spinning process to obtain a wire rod.", the wire-spinning temperature is 850-1000°C.
Citation Information
Patent Citations
Production method for manufacturing steel wire rod for X80 pipe line steel submerged arc welding wire
CN102161139A
Continuous-casting continuous-rolling method for producing sectional materials and bar-wire materials by using residual heat of molten steel
CN102310078A
Short-process long material endless rolling production line and short-process long material endless rolling method
CN110052495A
Method for rolling 635MPa-grade high-strength steel bar in short process by using waste heat of square billet