Method for differential-temperature ultrahigh-speed extrusion of magnesium alloy

Through the differential temperature ultra-high-speed extrusion method and the optimization design of alloy components, the problems of coarse grains and poor surface friction resistance caused by temperature rise in traditional isothermal extrusion are solved, and high-strength production is achieved. Ultra-high-speed extruded magnesium alloy improves production efficiency and mechanical properties.

CN118989018AActive Publication Date: 2024-11-22YANGZHOU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411320582.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-22
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

During the traditional isothermal extrusion process, the grain growth of magnesium alloys is caused by large temperature rise, which weakens the strengthening effect, poor surface friction resistance, and low extrusion speed, which limits the practical application of high-strength magnesium alloys.

Method used

By adopting the differential temperature ultra-high-speed extrusion method, the magnesium alloy ingot and the extrusion die are preheated to different temperatures respectively, so that the ingot temperature is 400℃, the mold temperature is 300℃, and the extrusion ratio is 278:1. The speed reaches 83 m/min, combined with the optimized design of the alloy components, a multi-component high-strength Mg-Bi-based alloy was prepared.

Benefits of technology

The ultra-high-speed extrusion forming of magnesium alloy is realized, which significantly improves production efficiency, refines the structure, improves strong plasticity and mechanical properties, overcomes the speed and strength limitations of traditional isothermal extrusion, and prepares high-strength, ultra-high-speed extrusion. New magnesium alloys pressed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989018A_ABST
    Figure CN118989018A_ABST
Patent Text Reader

Abstract

The invention discloses a method for differential-temperature ultrahigh-speed extrusion of a magnesium alloy, which comprises the following steps: carrying out differential-temperature extrusion deformation treatment on a solid-solution magnesium alloy, and then carrying out air cooling to room temperature to obtain a multi-component high-strength extruded Mg-Bi-based alloy; wherein the differential temperature extrusion deformation comprises the steps that a magnesium alloy cast ingot and an extrusion die are preheated for 2 h at the temperature of 400 DEG C and the temperature of 300 DEG C respectively; during extrusion, the ingot casting temperature is 400 DEG C, the mold temperature is 300 DEG C, the extrusion ratio is 278: 1, and the extrusion speed is 83 m / min. Through the synergistic effect of the alloy component optimization design and the differential temperature extrusion process, ultra-high-speed extrusion of the Mg-Bi-based alloy in the extrusion state is achieved, the extrusion speed reaches 83 m / min for the first time, and the production efficiency is greatly improved; and meanwhile, the structure is refined, synergistic improvement of strength and plasticity is achieved, preparation of the high-strength magnesium alloy capable of being extruded at the ultra-high speed is completed, and the method is superior to the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of engineering and material preparation, and in particular relates to a method for ultra-high speed extrusion of magnesium alloy at differential temperature. Background Art

[0002] Extrusion forming is a key process for manufacturing simple or complex shaped metal parts (such as plates, bars or profiles). Extruded alloys often show higher strength and ductility than cast alloys. For magnesium alloys, extrusion processing is conducive to obtaining fine grain structure of magnesium alloys and significantly improving the mechanical properties of magnesium alloys. However, the poor formability of magnesium alloys makes the extrusion speed low, which will undoubtedly increase production costs, reduce production efficiency, and limit the practical use of high-strength magnesium alloys.

[0003] In order to make magnesium alloy extruded products widely used in industry, it is necessary to achieve high strength and high extrudability at the same time. The research focus in recent years has been to develop high-strength magnesium alloys with excellent formability and ductility by introducing rare earth and other alloying elements to form RE-rich intermetallic phases. Although these intermetallic phases are crucial to strengthening the alloy during deformation processing, some of them will also significantly reduce the formability of the alloy, increase the deformation resistance of the alloy, and narrow the effective window of plastic processing; therefore, the effect of alloying on improving its extrudability is quite limited.

[0004] In the process of magnesium alloy extrusion, the traditional isothermal extrusion method is usually used to produce magnesium alloy products. In this method, the preheating temperature of the mold and the billet is the same, which causes a large temperature rise during the extrusion process, violent grain growth, coarse grains, and weakened grain boundary strengthening effect. In addition, magnesium alloys have low stress at high temperatures, poor surface friction resistance, and are prone to surface cracks at high temperatures.

[0005] Therefore, in order to make better use of extrusion technology, it is necessary to overcome the shortcomings of traditional isothermal extrusion and design a new high-strength magnesium alloy extrusion method that can be extruded at ultra-high speed. Summary of the invention

[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0008] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a magnesium alloy capable of ultra-high speed extrusion at differential temperature and a preparation method thereof. The high-strength and high-speed extruded magnesium alloy of the present invention has good strength and plasticity and ultra-high speed extrusion forming capability.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for ultra-high speed extrusion of magnesium alloy at differential temperature, comprising: The solid solution magnesium alloy is subjected to differential temperature extrusion deformation treatment and then air-cooled to room temperature to obtain a multi-component high-strength extruded Mg-Bi based alloy; The differential temperature extrusion deformation is to preheat the magnesium alloy ingot and the extrusion die at 400°C and 300°C for 2h respectively; The ingot temperature during extrusion was 400°C, the die temperature was 300°C, the extrusion ratio was 278:1, and the extrusion speed was 83 m / min.

[0010] As a preferred embodiment of the method of the present invention, the multi-component high-strength extruded Mg-Bi based alloy comprises, by mass percentage of each metal element, 5.0 wt.% Bi, 3.0 wt.% Al, 1.0 wt.% Zn, 0.2wt.% Mn, and the balance is magnesium.

[0011] As a preferred embodiment of the method of the present invention, the method for preparing a solid solution magnesium alloy comprises: According to the alloy component ratio, pure magnesium ingot, pure bismuth ingot, pure aluminum ingot, pure zinc particles and master alloy Mg-10Mn are selected as raw materials, and the raw materials are preheated at a first set temperature; Under the protection of SF6 and CO2, the pure magnesium is kept at the second set temperature, and then the temperature is raised to the third set temperature to melt the pure magnesium; adding pure bismuth ingots, pure aluminum ingots, pure zinc particles and master alloys, heating and melting, stirring and keeping warm at a fourth set temperature, blowing argon gas to perform refining and slag removal, and obtaining a multi-component micro-alloyed magnesium alloy melt; pouring the obtained multi-component micro-alloyed magnesium alloy melt into a steel mold to obtain a multi-component micro-alloyed magnesium alloy ingot; The obtained magnesium alloy ingot is cut into a Mg-Bi based alloy of a set size by wire electrode cutting, and then solution treated at a fifth set temperature and air-cooled to room temperature to obtain a solid solution magnesium alloy.

[0012] As a preferred embodiment of the method of the present invention, the first set temperature is 150° C. and the preheating treatment time is 90 minutes.

[0013] As a preferred embodiment of the method of the present invention, the second set temperature is 500° C. and the insulation time is 60 minutes.

[0014] As a preferred embodiment of the method of the present invention, the third set temperature is 750°C.

[0015] As a preferred embodiment of the method of the present invention, the fourth set temperature is 720° C. and the insulation time is 20 minutes.

[0016] As a preferred embodiment of the method of the present invention, the fifth set temperature is 450° C. and the insulation time is 12 hours.

[0017] Beneficial effects of the present invention: (1) The present invention, through the synergistic effect of alloy component optimization design and differential temperature extrusion process, not only realizes ultra-high-speed extrusion of extruded Mg-Bi-based alloy, but also achieves an extrusion speed of 83 m / min for the first time, greatly improving production efficiency; at the same time, it also refines the microstructure, achieves a synergistic improvement in strength and plasticity, and completes the preparation of high-strength magnesium alloy that can be extruded at ultra-high speed, which is superior to the existing technology.

[0018] (2) The present invention proposes for the first time a method for ultra-high-speed differential temperature extrusion of magnesium alloy. In contrast to the conventional isothermal extrusion process currently used, the present invention adopts the differential temperature extrusion process for the first time, breaking through the limitation of the extrusion speed in isothermal extrusion. The extrusion speed of magnesium alloy reaches 83 m / min for the first time. Generally speaking, increasing the extrusion speed will reduce the strength of the alloy, but the present invention achieves a synergistic improvement in extrusion speed, strength and plasticity, and has outstanding technical contributions. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them: Figure 1 are the macroscopic morphologies of Mg-Bi based alloys by differential temperature extrusion and isothermal extrusion; (a) and (b) are schematic diagrams of isothermal extrusion and differential temperature extrusion; (c), (d) and (e) are the macroscopic morphologies of Mg-Bi based alloys by isothermal extrusion and differential temperature extrusion, respectively; (f) and (g) are enlarged images of the selected area in (d); (h) is an enlarged image of the selected area in (g).

[0020] Figure 2 It is the 3D-Deform simulation process point tracking analysis and the corresponding temperature change diagram; among them, (a) is the 3D-Deform simulation isothermal process point tracking analysis diagram, (b) is the 3D-Deform simulation differential temperature ultra-high-speed extrusion process point tracking analysis diagram, and c) is the corresponding temperature change diagram.

[0021] Figure 3 is the electron backscattered diffraction image of the extruded Mg-Bi based alloy; where (a) and (b) are the EBSD images of the isothermal extrusion and differential temperature extrusion Mg-Bi based alloy, respectively, and (c) and (d) are the corresponding grain size distribution histograms.

[0022] Figure 4 It is the tensile engineering stress-strain curve of isothermal extrusion and differential temperature extrusion Mg-Bi based alloy. DETAILED DESCRIPTION

[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0024] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0025] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0026] The raw materials in the embodiments of the present invention are all common commercially available products.

[0027] Embodiment 1: Mg-5Bi-3Al-1Zn-0.2Mn (wt.%) was selected and prepared into a magnesium alloy according to the composition ratio. The preparation method includes the following steps: According to the alloy component ratio, pure magnesium ingot, pure aluminum ingot, pure zinc particles, master alloy Mg-10Bi (wt.%) and master alloy Mg-10Mn (wt.%) were selected as raw materials. According to the element mass percentage, Bi was 5.0 wt.%, Al was 3.0 wt.%, Zn was 1.0 wt.%, Mn was 0.2 wt.%, and the balance was magnesium. The raw materials were preheated at 150°C for 90 minutes; Under the protection of SF6 and CO2, the volume ratio of SF6 and CO2 is 1:99, and pure magnesium is kept at 500℃ for 60 minutes, and then heated to 750℃ to melt the pure magnesium; Pure aluminum ingots, pure zinc particles and three master alloys were added, heated and melted, stirred and kept at 720°C for 20 minutes, and then argon gas was blown in for refining and slag removal to obtain a multi-component microalloyed magnesium alloy melt; The obtained multi-component micro-alloyed magnesium alloy melt is poured into a Φ80×200 mm (diameter×height) steel mold (preheated to 350° C.) by gravity casting to obtain a multi-component micro-alloyed magnesium alloy ingot; The obtained magnesium alloy ingot was cut into a cast Mg-Bi based alloy with a diameter and a height of 80 mm and 80 mm respectively by wire electrode cutting, and after solution treatment, air-cooled to room temperature to obtain a solid solution Mg-Bi based alloy; The obtained solid solution Mg-Bi based alloy is subjected to extrusion deformation treatment and then air-cooled to room temperature to obtain a multi-component extruded Mg-Bi based alloy.

[0028] Before extrusion deformation, the solid solution Mg-Bi based alloy and the extrusion die were preheated at 400°C and 300°C for 2h, respectively, and then extruded at an extrusion ratio of 278:1 and a speed of 83 m / min.

[0029] Embodiment 2: The difference between this embodiment and embodiment 1 is that before extrusion deformation, the solid solution Mg-Bi based alloy and the extrusion die are preheated at 400° C. for 2 h, and then extrusion is performed at an extrusion ratio of 278:1 and a speed of 83 m / min.

[0030] Figure 1 (a) and (b) show schematic diagrams of isothermal extrusion and differential temperature extrusion. In isothermal extrusion, the die temperature is the same as the ingot temperature, while in differential temperature extrusion, the die temperature is lower than the ingot temperature. The macroscopic morphology of the alloys under the two extrusion methods was observed. Figure 1 ce), despite the large deformation, the alloys can be successfully extruded in both methods. It is worth noting that a large number of thermal cracks appear on the surface of the alloy produced by isothermal extrusion, as shown in the enlarged figure. Figure 1 As shown in (f, g), the alloy produced by differential temperature extrusion has good surface quality, smooth and without cracks.

[0031] The generation of hot cracks is mainly due to the increase in extrusion temperature under high-speed extrusion conditions, which makes the thermally unstable phase easily dissolve into the matrix.

[0032] Figure 2 The 3D-Deform simulation shows the point tracking analysis of (a) isothermal and (b) differential temperature ultra-high-speed extrusion processes. The temperature during isothermal extrusion is significantly higher than that during differential temperature extrusion. The corresponding temperature changes during the extrusion process are analyzed by point tracking ( Figure 2c) As the extrusion process proceeds, the alloy temperature under the two extrusion methods first increases gradually and then increases rapidly. The temperature during isothermal extrusion is as high as 573°C, which is higher than the peak temperature of 561°C in the DSC spectrum. During differential temperature extrusion, the die temperature is lower, which limits the temperature rise during extrusion, with a maximum of 534°C. Compared with isothermal extrusion, the temperature is reduced by about 40°C, which is significantly lower than the peak temperature in the DSC spectrum, providing a guarantee for ultra-high-speed extrusion of the alloy.

[0033] Samples with a length of 7×5×3 mm were processed from the two extruded bars along the extrusion direction. The samples were ground, cleaned and blown dry, and electropolished for 90 s using AC2 special electrolyte under the conditions of voltage 20 V, current 0.03 A and temperature -25 °C. The EBSD results are shown in Figure 2. Figure 3 As shown in the figure, both extruded alloys show a completely recrystallized structure and basal fiber texture. The alloy produced by differential temperature extrusion has a smaller grain size (15.2μm) and a weaker texture strength (8.1). This is due to the significant temperature difference between the ingot and the extrusion die, which promotes the refinement of the structure.

[0034] Tensile specimens with a size of 5×25 mm were processed from the two extruded bars along the extrusion direction, and tensile tests were carried out along the extrusion direction at room temperature. Each tensile test was carried out three times to ensure the accuracy of the experiment. Its mechanical properties are as follows Figure 4 As shown in the figure, the yield strength, tensile strength and elongation (283MPa, 331Mpa and 19.0%) of the differential temperature extruded alloy are higher than those of the isothermal extruded alloy (270MPa, 306Mpa and 12.6%). Under ultra-high-speed extrusion of 83m / min, the synergistic improvement of yield strength and tensile plasticity is achieved, and the preparation of a new high-strength magnesium alloy that can be extruded at ultra-high speed is realized.

[0035] Embodiment 3: The difference between this embodiment and embodiment 1 is that before extrusion deformation, the solid solution Mg-Bi based alloy and the extrusion die are preheated at 310° C. for 2 h, and then extrusion is performed at an extrusion ratio of 28:1 and a speed of 73 m / min.

[0036] A tensile specimen with a size of 5×25 mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0037] Comparative Example 1: The difference from Example 2 is that the content of Zn element in the alloy is 0, and the alloy composition includes 5.0 wt.% Bi, 3.0 wt.% Al, 0.2 wt.% Mn, and the balance is magnesium.

[0038] Before extrusion deformation, the solid solution Mg-Bi based alloy and the extrusion die were preheated at 400℃ for 2h, and then extruded at an extrusion ratio of 76.5:1 and a speed of 67 m / min. A tensile specimen with a size of Ф5×25mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0039] Comparative Example 2: Mg-5Bi-2Al-0.2Mn (wt.%) was selected. The difference from Comparative Example 1 is that the Al element content in the alloy is 2.0wt.%, and the alloy components include 5.0 wt.% Bi, 0.2 wt.% Mn, and the balance is magnesium.

[0040] Before extrusion deformation, the solid solution Mg-Bi based alloy and the extrusion die were preheated at 400 °C for 2 h, and then extruded at an extrusion ratio of 76.5:1 and a speed of 70 m / min.

[0041] A tensile specimen with a size of 5×25 mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0042] Comparative Example 3: Mg-3Bi-8Al (wt.%) alloy was selected and solution treated at 390 °C for 12 h; Then, the solution treated ingot and mold were preheated at 300℃ for 30min, and then extruded at an extrusion ratio of 25:1 and a speed of 6m / min. A tensile specimen with a size of Ф5×25mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0043] Comparative Example 4: A high rare earth content Mg-10.3Gd-4.4Y-0.9Zn-0.7Mn (wt.%) alloy was selected and subjected to a multi-stage solution treatment, i.e., heating at 450 °C for 8 h, then heating at 500 °C for 8 h, and then heating at 525 °C for 5 h.

[0044] Before extrusion deformation, the solution treated ingot and mold were preheated at 510℃ and 390℃ for 30min respectively, and then extruded at an extrusion ratio of 11:1 and a speed of 1.3 m / min. A tensile specimen with a size of Ф5×25mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0045] Comparative Example 5: The difference between this comparative example and comparative example 3 is that before extrusion deformation, the solution treated ingot and the mold are preheated at 450° C. for 30 min, and then extrusion is performed at an extrusion ratio of 11:1 and a speed of 0.2 m / min.

[0046] A tensile specimen with a size of 5×25 mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0047] Comparative Example 6: The difference between this comparative example and comparative example 3 is that before extrusion deformation, the solution treated ingot and the mold are preheated at 510°C and 450°C for 30 minutes respectively, and then extrusion is carried out at an extrusion ratio of 11:1 and a speed of 1.3 m / min.

[0048] A tensile specimen with a size of 5×25 mm was processed from the extruded bar along the extrusion direction, and a tensile test was performed along the extrusion direction at room temperature. Each tensile test was performed three times to ensure the accuracy of the experiment.

[0049] The mechanical properties and extrusion parameters of the magnesium alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 6 are as follows:

[0050] From the above, it can be seen that the present invention uses the synergistic effect of alloy component optimization design and differential temperature extrusion process to promote microstructure refinement by utilizing the significant temperature difference between the ingot and the extrusion die, thereby achieving a synergistic improvement in strength and plasticity and extrusion speed. Compared with the isothermal extrusion at 400°C in Example 2, the higher ingot temperature during the differential temperature extrusion process softens the alloy, while the lower extrusion die temperature leads to a limited temperature rise. The extrusion speed of the obtained Mg-Bi-Al-Zn alloy reaches 83m / min for the first time, and the surface quality of the bar is good, smooth and crack-free; at the same time, the fine grain structure enhances the strength and plasticity of the alloy, and realizes the preparation of high-strength magnesium alloys that can be extruded at ultra-high speed. Generally speaking, lowering the extrusion temperature is beneficial to improving the strength of the alloy. Although the alloy in Example 3 is extruded at a low temperature of 310°C, its strength and plasticity and extrusion speed are still lower than those of the present invention.

[0051] Compared with comparative examples 1-6, the present invention improves the comprehensive mechanical properties of the alloy while improving the extrusion speed by optimizing the alloy composition design. Even compared with high rare earth content alloys, it still has great advantages. The addition of a large amount of rare earth elements will significantly improve the mechanical properties of the alloy, but it will undoubtedly increase the material cost. In addition, the extrusion speed of the high rare earth content magnesium alloy in the comparative example is relatively low. Even if the differential temperature extrusion technology is adopted, the extrusion speed is only 1.3m / min, which is much lower than 83m / min of the present invention, which is not conducive to large-scale industrial production. In summary, the present invention helps to improve the problem of poor plastic deformation ability of magnesium alloys, improve processing efficiency, and expand the scope of industrial application by optimizing the alloy component design and adopting the differential temperature extrusion process.

[0052] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A method for ultra-high speed extrusion of magnesium alloy at differential temperature, characterized in that: include, The solid solution magnesium alloy is subjected to differential temperature extrusion deformation treatment and then air-cooled to room temperature to obtain a multi-component high-strength extruded Mg-Bi based alloy; The differential temperature extrusion deformation is to preheat the magnesium alloy ingot and the extrusion die at 400°C and 300°C for 2h respectively; The ingot temperature during extrusion was 400°C, the die temperature was 300°C, the extrusion ratio was 278:1, and the extrusion speed was 83 m / min.

2. The method according to claim 1, characterized in that: The multi-component high-strength extruded Mg-Bi based alloy includes, by weight percentage of each metal element, 5.0 wt.% Bi, 3.0 wt.% Al, 1.0 wt.% Zn, 0.2 wt.% Mn, and the balance is magnesium.

3. The method according to claim 1 or 2, characterized in that: The method for preparing the solid solution magnesium alloy comprises: According to the alloy component ratio, pure magnesium ingot, pure bismuth ingot, pure aluminum ingot, pure zinc particles and master alloy Mg-10Mn are selected as raw materials, and the raw materials are preheated at a first set temperature; Under the protection of SF6 and CO2, the pure magnesium is kept at the second set temperature, and then the temperature is raised to the third set temperature to melt the pure magnesium; adding pure bismuth ingots, pure aluminum ingots, pure zinc particles and master alloys, heating and melting, stirring and keeping warm at a fourth set temperature, blowing argon gas to perform refining and slag removal, and obtaining a multi-component micro-alloyed magnesium alloy melt; pouring the obtained multi-component micro-alloyed magnesium alloy melt into a steel mold to obtain a multi-component micro-alloyed magnesium alloy ingot; The obtained magnesium alloy ingot is cut into a Mg-Bi based alloy of a set size by wire electrode cutting, and then solution treated at a fifth set temperature and air-cooled to room temperature to obtain a solid solution magnesium alloy.

4. The method according to claim 3, characterized in that: The first set temperature is 150° C., and the preheating treatment time is 90 minutes.

5. The method according to claim 3, characterized in that: The second set temperature is 500° C., and the holding time is 60 min.

6. The method according to claim 3, characterized in that: The third set temperature is 750°C.

7. The method according to claim 3, characterized in that: The fourth set temperature is 720° C., and the insulation time is 20 minutes.

8. The method according to claim 3, characterized in that: The fifth set temperature is 450° C., and the heat preservation time is 12 hours.

Citation Information

Patent Citations

  • High-speed-extrudable wrought magnesium alloy and preparation method thereof

    CN105154734A

  • High-toughness magnesium alloy deformation material and preparation method thereof

    CN115478199A

  • Heat-resistant magnesium alloy capable of being extruded at high speed and preparation method thereof

    CN117286379A

  • Magnesium alloy with excellent extrusion processability and high plasticity and preparation method thereof

    CN117448642A

  • Low-cost microalloyed high-performance rapidly-extruded magnesium alloy and preparation method thereof

    CN117904505A