Narrow-face copper plate, working face design method of narrow-face copper plate and crystallizer

By designing the working face of narrow-side copper plate with asymmetric structure, the problems of edge cracks, inverted trapezoidal shapes and corner defects in the casting process are solved, and the efficient uniform solidification of the casting billet and the long life of the crystallizer are achieved, which improves the The yield and production efficiency of wide and thick plates.

CN118989258APending Publication Date: 2024-11-22NORTHEASTERN UNIV CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410788228.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing narrow-side copper plates have edge cracks, inverted trapezoidal structures and corner defects in the casting process, resulting in low material yield and poor production efficiency of wide and thick plates, and short service life of the crystallizer.

Method used

Design a narrow-sided copper plate working surface with an asymmetric structure, and ensure that the slope difference between the first convex surface and the second convex surface is set, combining taper compensation and convex curve expressions. The arc is narrow and the outer arc is wide, which avoids additional occupation in the transition zone between the middle and the edges, meets the solidification and shrinkage characteristics of the casting blank, and achieves efficient and uniform solidification of the casting blank.

Benefits of technology

Effectively reduce the edge defects of wide and thick plates, improve the yield and production efficiency, reduce the occurrence of cracks in the corners of the casting blank, extend the service life of the crystallizer, and ensure the good fit of the casting blank with the copper plate during the entire solidification process. and uniform heat transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989258A_ABST
    Figure CN118989258A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal casting, and particularly provides a narrow-face copper plate, a working face design method of the narrow-face copper plate and a crystallizer. The narrow-face copper plate is applied to the crystallizer, the crystallizer is provided with an inner cavity used for solidifying molten steel into a casting blank, and the narrow-face copper plate comprises a working face which is of a curved surface structure protruding towards the inner cavity; the working face comprises a first convex face and a second convex face, the first convex face is arranged on one side of the transverse center line of the narrow-face copper plate, the second convex face is arranged on the other side of the transverse center line of the narrow-face copper plate, and the protruding heights of the first convex face and the second convex face are gradually reduced in the direction away from the transverse center line of the narrow-face copper plate. The gradient of the first convex surface is smaller than that of the second convex surface. According to the narrow-face copper plate, the edge protruding height of the first convex face is larger than that of the second convex face, so that the inner arc is narrow and the outer arc is wide when a narrow-face inwards-concave casting blank produced by the crystallizer applying the narrow-face copper plate is discharged out of a lower opening of the crystallizer, and it can be guaranteed that the inner arc width and the outer arc width are equal after the narrow-face inwards-concave casting blank is discharged out of a straightening area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of metal casting, and specifically relates to a narrow copper plate, a working surface design method of the narrow copper plate, and a crystallizer. Background Art

[0002] During the preparation of wide and thick plates, the edges of the wide and thick plates have a high incidence of edge crack defects (called "edge straight cracks" or "edge black lines" in the industry) in a wide range of 45 to 120 mm, which seriously restricts the high-quality and high-yield production of wide and thick plates. At the same time, the slabs required for continuous casting and rolling of wide and thick plates have an inverted trapezoidal structure with a wide upper surface and a narrow lower surface after the straightening process, resulting in the steel plates after rolling also having a wide upper surface and a narrow lower surface shape, further increasing the amount of defects removed from the edges of the wide and thick plates, causing huge economic losses to users, which is a difficult problem that needs to be overcome in the preparation of wide and thick plates.

[0003] For edge cracks, a large number of practices have shown that the width of edge cracks can be effectively reduced by preparing slabs with narrow faces, large arc surfaces and concave structures (concave arc span / slab thickness ≥ 0.8, concave amount ≥ 10 mm). If the problem of the continuous casting slab being in an inverted trapezoidal shape after the straightening process can be further solved on the basis of preparing narrow concave slabs, the trimming width of the edges of wide and thick plates can be greatly reduced, and the yield rate of wide and thick plates can be significantly improved. To this end, based on the continuous casting crystallizer, preparing a slab with a narrow inner arc (i.e., the upper surface of the slab), a wide outer arc (the lower surface of the slab), and a narrow face with a large arc concave structure from the source is an effective way to solve the above-mentioned problems.

[0004] In order to prepare narrow concave billets, Chinese utility model patent CN204997018U and Chinese invention patent CN106270433B proposed a crystallizer with a convex block structure in the middle of the narrow copper plate in the width direction. In the above two prior arts, the middle convex block of the narrow copper plate is an arc structure, and the edge is a horizontal base surface, and the two are transitioned by tangency. However, in the actual implementation process, the arc convex block and the horizontal base surface of the edge cannot be tangent. In order to achieve a smooth tangent transition between the two interfaces, a transition arc tangent to the two is additionally introduced at the junction of the arc convex block and the horizontal base surface of the edge. Affected by the excessive width occupied by the transition arc and the horizontal base surface of the edge of the copper plate, the width of the arc convex block in the middle of the copper plate is greatly reduced, which cannot meet the requirement of effectively controlling the width of the edge crack and the concave arc surface span of the narrow face of the billet / bill thickness ≥ 0.8. At the same time, in the actual implementation process of the above two existing technologies, due to the combined effects of the large and rapid concave in the middle of the narrow surface of the ingot during the solidification process and the pressure reduction at the end of solidification, the middle of the narrow surface of the ingot presents an obvious nearly "triangular" concave structure, which causes the ingot to form double-strand shape defects on both sides of the thickness centerline during the actual rolling process, and even deep folding line defects in the middle of the thickness of the wide and thick plate.

[0005] In view of the defects of Chinese utility model patent CN204997018U and Chinese invention patent CN106270433B, Chinese utility model patent CN214349470U and Chinese invention patent CN112846116A proposed a crystallizer with a narrow face as a full arc face. That is, the working surface of the narrow copper plate of the crystallizer is designed from top to bottom as an arc-shaped structure with the same radius in the horizontal direction, and the highest protrusion height of the arc surface is 10 to 20 mm, thereby realizing the preparation of a casting blank with a narrow face, a large arc face, and a large inner concave structure. However, since the working surface of the narrow copper plate in the above two prior arts is the same arc-shaped structure from the upper mouth to the lower mouth, the corner of the casting blank formed by the solidification of the molten steel in the crystallizer has an obvious sharp angle structure (the narrow face transverse arc copper plate and the flat wide copper plate form an acute angle). Affected by this, on the one hand, the heat transfer rate of the corners of the ingot with the sharp-angle structure in the secondary cooling casting zone is significantly accelerated, so that when producing continuous casting ingots of micro-alloyed steel containing Nb, V, Al, etc., the ingot is prone to transverse crack defects at the corners due to the excessively low corner temperature when passing through the straightening zone; on the other hand, the narrow copper plate of the crystallizer adopts the same arc-shaped structure from top to bottom horizontally. Under the action of solidification shrinkage, the corners of the ingot with the sharp-angle structure separate from the copper plate prematurely to form a large gap, which causes the formation of coarse austenite grains at the corners of the ingot shell, which is also not conducive to the control of cracks at the corners of the ingot.

[0006] In view of the defects of Chinese utility model patent CN214349470U and Chinese invention patent CN112846116A, Chinese invention patent CN115815545A proposes a crystallizer with a transition structure in which the convex arc in the middle is directly connected to the straight edge area, thereby ensuring the preparation of a narrow-surface, large-arc, large-indentation, right-angled structure of a casting blank, significantly reducing the width of the edge crack, while also ensuring that the corner temperature of the casting blank during the solidification process in the casting stream in the second cooling zone is not lower than the corner of the traditional narrow-surface flat casting blank, effectively reducing the occurrence of cracks in the corner of the casting blank. However, since the middle arc surface and the straight edge area of ​​the copper plate in the prior art are directly intersected to transition, the actual solidification process is affected by the surface tension of the molten steel and the liquid protective slag, and the solidified blank shell at the intersection transition zone cannot fit with the copper plate for heat transfer due to the sudden convexity of the middle arc surface, which easily leads to a steel leakage accident in the transition zone due to the excessive thinness of the solidified blank shell.

[0007] The crystallizer of Chinese invention patent CN117139575A further introduces an arc transition zone at the junction of the central convex arc and the edge straight zone on the basis of the crystallizer of Chinese invention patent CN115815545A. The effect of this method is reduced to the disadvantage of the crystallizer of Chinese utility model patent CN204997018U and Chinese invention patent CN106270433B, that is, the solidification process of the billet is prone to form a "triangular" concave structure in the middle of the narrow surface of the billet due to the excessive width occupied by the edge straight zone and the transition zone.

[0008] Chinese invention patent CN112118924A discloses a crystallizer for compensating for the shrinkage of the shell during solidification in the crystallizer. Although its narrow copper plate also proposes a convex arc structure, the height of the protrusion gradually decreases from the upper mouth to the lower mouth of the crystallizer, and is even reduced to a flat structure. That is, the crystallizer structure cannot produce a narrow concave slab.

[0009] In order to solve the problem that the slab forms an inverted trapezoidal structure after the straightening process, Chinese utility model patents CN209531721U and CN213614019U propose a casting blank holding device at the exit of the fan-shaped segment, which squeezes the narrow surface of the slab through the holding roller to make the narrow surface flush.

[0010] On the basis of CN117139575A, the Chinese invention patent CN117961017A retains the structure of the inner arc side with straight edge, transition arc and circular arc in sequence, and the outer arc side of the copper plate is designed as a wider crystallizer cavity structure than the inner arc side through the inclined section. However, the outer arc of the billet produced by this method has a significant sharp angle structure, which makes it very easy to produce corner transverse cracks in the billet during bending and other processes.

[0011] In addition, the arc-shaped working surfaces of the crystallizers of the above-mentioned Chinese utility model patent CN204997018U, Chinese invention patent CN106270433B, Chinese utility model patent CN214349470U, Chinese invention patent CN112846116A, CN117139575A, and CN117961017A do not take into account the shrinkage of the billet in the thickness direction in the crystallizer. In the actual slab continuous casting process, the billet solidifies in the crystallizer, and shrinks by 1 to 3 mm in the thickness direction. That is, the width of the narrow copper plate of the actual crystallizer is linearly reduced by 1 to 3 mm from the upper mouth to the lower mouth. In the above-mentioned developed crystallizers of this type, whether the working surface is designed with the same convex block in the middle or the same arc structure, the actual solidification characteristics of the billet are not taken into account. The contraction of the billet along the thickness direction during the solidification process will "lock" the two sides of the protrusion or arc in the middle of the crystallizer, thereby greatly wearing out the two sides of the arc surface in the middle and lower part of the copper plate and preventing it from serving for a long time. Although the copper plate of Chinese invention patent CN115815545A takes this problem into consideration, it converts all the solidification contraction of the billet along the thickness direction into the reduction of the span of the middle arc, that is, it does not consider the contraction of the straight edge area. This causes the concave arc surface of the billet at the intersection of the straight edge area and the middle arc to separate from the arc side of the copper plate during the solidification process of the billet, further exacerbating the risk of steel leakage in the boundary area of ​​the billet.

[0012] In addition, the above-mentioned convex crystallizers for preparing narrow concave slabs have not considered the nonlinear change in the height direction of the shrinkage of the billet in the width direction in the crystallizer, that is, the billet shrinks faster in the width center direction in the middle and upper part of the crystallizer, and shrinks relatively slowly in the middle and lower part. In the narrow concave billet prepared by the above-mentioned developed crystallizer, the billet cannot obtain the efficient support and heat transfer of the narrow copper plate during the solidification process in the middle and upper part of the crystallizer, and the grain structure of the corner of the billet is often coarse, and the proportion of corner crack defects in the actual production process is high; while in the middle and lower part of the crystallizer, the billet shell with slowed shrinkage and the narrow copper plate form mutual extrusion, which aggravates the wear of the copper plate in the middle and lower part of the crystallizer.

[0013] To this end, taking into account the edge cracks of wide and thick plates, the control effect of inverted trapezoidal shape of the ingot, the quality of the ingot corners, and the service life of the crystallizer, it is urgent to develop a narrow copper plate that can be used in the crystallizer to simultaneously meet the production of ingots with narrow inner arc, wide outer arc, narrow face, large arc surface, large inner concave amount and no defects in the corners, while taking into account long service life. Summary of the invention

[0014] Therefore, the technical problem to be solved by the present application is to provide a narrow-face copper plate, a working surface design method for a narrow-face copper plate and a crystallizer, wherein the working surface of the narrow-face copper plate is an asymmetric structure, and the edge protrusion height of the first convex surface is greater than the edge protrusion height of the second convex surface, so that the inner arc and outer arc of the ingot produced by the crystallizer using the narrow-face copper plate are narrow and wide, which can ensure that the difference in inner and outer arc widths is less than 3 mm after the ingot leaves the straightening zone, thereby further reducing the amount of steel plate trimming.

[0015] In order to solve the above problems, in a first aspect of the present application, a narrow copper plate is provided, which is applied to a crystallizer, wherein the crystallizer has an inner cavity for solidifying molten steel into a cast billet, and the narrow copper plate includes a working surface, which is a curved surface structure convex toward the inner cavity, and the working surface of the curved surface structure conforms to the formula:

[0016] D=D1+D2

[0017] Wherein, D1 is the expression of the taper compensation value of the working surface in the height direction of the narrow copper plate; D2 is the expression of the convex curve of the working surface in the width direction of the narrow copper plate;

[0018] Among them, the working surface includes a first convex surface and a second convex surface. The first convex surface is arranged on one side of the transverse center line of the narrow copper plate, and the second convex surface is arranged on the other side of the transverse center line of the narrow copper plate. The protrusion heights of the first convex surface and the second convex surface gradually decrease in the direction away from the transverse center line of the narrow copper plate, and the slope of the first convex surface is smaller than the slope of the second convex surface.

[0019] Optionally, the edge of the first convex surface away from the second convex surface is the first contour line, and the edge of the second convex surface away from the first convex surface is the second contour line. At the same height, the difference between the protrusion height of the first contour line and the protrusion height of the second contour line is Δh, 3mm≤Δh≤20mm.

[0020] Optionally, at the height of the top surface of the narrow copper plate, the difference between the protrusion height of the transverse center line of the narrow copper plate and the protrusion height of the first contour line is B1, 5mm≤B1≤20mm.

[0021] Optionally, the taper compensation value expression of the working surface in the height direction of the narrow copper plate conforms to the formula:

[0022]

[0023] In the formula, A i is the fitting coefficient of the seventh-order polynomial; y is the distance from the top surface of the narrow copper plate.

[0024] Optionally, the convex curve expression of the working surface in the width direction of the narrow copper plate conforms to the formula:

[0025]

[0026] In the formula, x is the position relative to the transverse center line of the narrow copper plate in the width direction of the narrow copper plate. When x is a negative value, it is located on the first convex surface, and when x is a positive value, it is located on the second convex surface; B2 is the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate; B3 is the taper compensation correction value of the working surface of the narrow copper plate in the height direction.

[0027] Optionally, the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate conforms to the formula:

[0028]

[0029] Where l1 is the height of the narrow copper plate.

[0030] Optionally, the taper compensation correction value of the working surface of the narrow copper plate in the height direction conforms to the formula:

[0031]

[0032] Where l2 is the width of the top surface of the narrow copper plate; y0 is the y value when D1 takes the maximum value.

[0033] Optionally, in the height direction of the narrow copper plate, the width of the narrow copper plate decreases linearly by 1 to 3 mm from the top surface to the bottom surface.

[0034] In a second aspect of the present application, a method for designing a working surface of a narrow copper plate is provided, which is used to design the working surface of any of the above narrow copper plates, and the method comprises:

[0035] Step 1: Obtain high temperature thermal / mechanical properties of steel and thermal properties of the mold copper plate and cooling water;

[0036] Step 2: Using the direct fluid-solid coupling algorithm, calculate the solidification shrinkage of the ingot from the corner to the center of the wide surface in the crystallizer with the working surface of the narrow copper plate as a plane structure;

[0037] Step 3: Based on the distribution of the solidification shrinkage from the corner of the ingot to the center of the wide surface of the crystallizer in the height direction of the crystallizer, determine the expression of the taper compensation value of the working surface in the height direction of the narrow copper plate;

[0038] Step 4: Based on the height and width of the narrow copper plate, determine the convex curve expression of the working surface in the width direction of the narrow copper plate;

[0039] Step 5: Based on the expression of the taper compensation value of the working surface in the height direction of the narrow copper plate and the expression of the convex curve of the working surface in the width direction of the narrow copper plate, determine the surface expression of the working surface.

[0040] The third aspect of the present application provides a crystallizer, comprising any one of the narrow copper plates mentioned above, wherein two narrow copper plates are arranged opposite to each other, and the crystallizer also comprises two oppositely arranged wide copper plates, and the combination of the two oppositely arranged wide copper plates and the two oppositely arranged narrow copper plates is suitable for forming an inner cavity for solidifying molten steel into a cast billet.

[0041] Beneficial effects:

[0042] The embodiment of the present invention provides a narrow copper plate, a working surface design method of a narrow copper plate and a crystallizer, wherein the narrow copper plate sets the slope of the first convex surface to be smaller than the slope of the second convex surface, so that the inner arc of the ingot produced by the crystallizer prepared by the narrow copper plate is narrow and the outer arc is wide, ensuring that the widths of the inner and outer arcs of the ingot after passing the straightening zone are equivalent, further reducing the trimming amount of the steel plate, and improving the yield rate of the wide and thick plate; at the same time, by setting the convex area in the middle of the working surface of the narrow copper plate and the nearly straight area at the edge, the convex area in the middle to the nearly straight area at the edge are continuously and smoothly transitioned as a whole, avoiding the need to set an additional transition area for the transition between the middle and the edge of the working surface, resulting in the additional introduction of the transition area making the span of the central convex area too small, thereby failing to effectively reduce the width of the edge crack defect of the ingot during the rolling process and causing the defect of the double-strand shape, and also avoiding the problem of leakage of the solidified ingot shell due to the lack of a smooth transition area between the middle and the edge of the working surface, ensuring that the crystallizer can prepare narrow faces with large arcs and large inner concave surfaces with high quality. The billet with nearly right-angle structure at the corner can reduce the width of the wide side crack of the wide and thick plate, and ensure the high-temperature over-straightening of the corner of the billet in the second cooling zone to prevent the occurrence of cracks in the corner of the billet; at the same time, the adjustment factor is introduced into the span of the central convex surface of the working surface of the narrow copper plate, so that the span of the central convexity and the width of the nearly straight area of ​​the edge can be adjusted along with the shrinkage characteristics of the billet during the solidification, thereby ensuring that the concave surface of the narrow surface of the billet fits well with the working surface of the narrow copper plate throughout the solidification process, and the solidification is highly fitted in the horizontal direction. While the ingot solidifies efficiently and evenly, the wear on both sides of the raised arc surface in the middle of the copper plate is reduced, and the service life of the crystallizer is improved; the working surface of the narrow copper plate is designed along its height direction as a curved taper compensation structure that caters to the solidification shrinkage characteristics of the ingot shell, which meets the characteristics of the dynamic solidification of the ingot in the height direction, ensuring that the narrow surface of the ingot fits well with the copper plate during the entire solidification process, so that the heat transfer between the two is uniform; in addition, the compensation correction value considering wear is introduced in the nearly straight edge area of ​​the working surface of the narrow copper plate, see Figure 4 and Figure 5 As shown, the taper compensation value of the nearly straight area of ​​the edge of the working surface at a height below the maximum taper compensation value in the height direction gradually decreases, which solves the problem of severe wear of the edge of the lower area of ​​the crystallizer in the actual continuous casting process. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a schematic structural diagram of a narrow copper plate of an optional embodiment of the present application;

[0044] Figure 2 A topographical diagram of a working surface of a narrow copper plate of an optional embodiment of the present application without considering D1;

[0045] Figure 3 A transverse cross-sectional view of a narrow copper plate of an optional embodiment of the present application;

[0046] Figure 4This is a comparison diagram of the edge contour lines of the first convex surface at a height of 312 mm from the top surface of the narrow copper plate and at the lower mouth of the crystallizer in an optional embodiment of the present application;

[0047] Figure 5 This is a comparison diagram of the edge contour lines of the second convex surface at a height of 312 mm from the top surface of the narrow copper plate and at the lower mouth of the crystallizer in an optional embodiment of the present application;

[0048] Figure 6 A flow chart of a method for designing a working surface of a narrow copper plate according to an optional embodiment of the present application;

[0049] Figure 7 A flow chart of a method for designing a working surface of a narrow copper plate according to another optional embodiment of the present application;

[0050] Figure 8 This is a schematic structural diagram of a crystallizer according to an optional embodiment of the present application.

[0051] The reference numerals are as follows:

[0052] 100, narrow copper plate; 200, wide copper plate; 300, casting billet;

[0053] 1. Working surface; 11. First convex surface; 111. First contour line; 12. Second convex surface; 121. Second contour line; 2. Top surface; 3. Horizontal center line of narrow copper plate. DETAILED DESCRIPTION

[0054] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0055] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0056] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0057] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0058] See also Figures 1 to 5 As shown, according to the first aspect of an embodiment of the present application, a narrow copper plate 100 is provided, which is applied to a crystallizer. The crystallizer has an inner cavity for solidifying molten steel into a cast billet 300. The narrow copper plate 100 includes a working surface 1, which is a curved surface structure convex toward the inner cavity; the working surface 1 includes a first convex surface 11 and a second convex surface 12, the first convex surface 11 is arranged on one side of the transverse center line 3 of the narrow copper plate, and the second convex surface 12 is arranged on the other side of the transverse center line 3 of the narrow copper plate, and the convex heights of the first convex surface 11 and the second convex surface 12 gradually decrease in the direction away from the transverse center line 3 of the narrow copper plate, and the slope of the first convex surface 11 is smaller than the slope of the second convex surface 12.

[0059] Among them, the working surface 1 of the curved structure conforms to the formula:

[0060] D=D1+D2 (1)

[0061] Wherein, D1 is the expression of the taper compensation value of the working surface 1 in the height direction of the narrow copper plate 100; D2 is the expression of the convex curve of the working surface 1 in the width direction of the narrow copper plate 100.

[0062] The taper compensation value expression of the working surface 1 in the height direction of the narrow copper plate 100 conforms to the formula:

[0063]

[0064] In the formula, A i is the fitting coefficient of the seventh-order polynomial; y is the distance from the top surface of the narrow copper plate.

[0065] The convex curve expression of the working surface in the width direction of the narrow copper plate conforms to the formula:

[0066]

[0067] In the formula, x is the position relative to the transverse center line 3 of the narrow copper plate in the width direction of the narrow copper plate 100, and is located on the first convex surface 11 when x is a negative value, and is located on the second convex surface 12 when x is a positive value; B1 is the height difference between the raised height of the transverse center line 3 of the narrow copper plate and the raised height of the first contour line 111 at the height of the top surface 2 of the narrow copper plate 100, and the value range is 5 to 20 mm; B2 is the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface 1 of the narrow copper plate 100; B3 is the taper compensation correction value of the working surface 1 of the narrow copper plate 100 in the height direction.

[0068] The adjustment factor of the transverse span of the middle raised area in the width direction of the working surface 1 of the narrow copper plate 100 conforms to the formula:

[0069]

[0070] The taper compensation correction value of the working surface 1 of the narrow copper plate 100 in the height direction conforms to the formula:

[0071]

[0072] Wherein, l2 is the width of the top surface 2 of the narrow copper plate 100; y0 is the y value when D1 takes the maximum value.

[0073] Among them, the narrow copper plate 100 provided in the embodiment of the present application can be applied to a crystallizer to produce a narrow concave casting billet 300 with a narrow inner arc, a wide outer arc, a large narrow face span, a large inner concave amount, a nearly right-angle structure at the corner, and no defects. It should be noted that the inner arc can be the upper surface of the casting billet 300, and the outer arc can be the lower surface of the casting billet 300.

[0074] For details, see Figure 8 As shown, two wide copper plates 200 and two narrow copper plates 100 are combined to form a crystallizer cavity, which is used to solidify molten steel into a billet shell, and to continuously cast and produce a narrow concave billet 300 with a narrow arc, a wide outer arc, a large narrow span, a large inner concave amount, a nearly right-angle structure at the corner, and no defects. It can be understood that the transverse direction of the narrow copper plate 100 is the width direction of the narrow copper plate 100, and the width direction of the narrow copper plate 100 is the thickness direction of the billet 300, that is, the transverse direction of the narrow copper plate 100 is the thickness direction of the billet 300.

[0075] The wide copper plate 200 may be a flat copper plate, and the narrow copper plate 100 may be a convex curved copper plate.

[0076] The narrow copper plate 100 includes a top surface 2 and a bottom surface, the top surface 2 of the narrow copper plate 100 is flush with the upper opening of the crystallizer, and the bottom surface of the narrow copper plate 100 is flush with the lower opening of the crystallizer. It can be understood that the upper opening of the crystallizer can be an end where the molten steel enters the inner cavity of the crystallizer, and the lower opening of the crystallizer can be an end where the ingot 300 leaves the inner cavity of the crystallizer.

[0077] The narrow copper plate 100 further includes a working surface 1, which may be the wall of the narrow copper plate 100 facing the inner cavity of the crystallizer, that is, the working surface 1 is the wall of the narrow copper plate 100 in contact with the solidified ingot 300.

[0078] Specifically, the working surface 1 is convex toward the inner cavity of the crystallizer, and the working surface 1 is a convex surface. The expression of the convex surface conforms to Formula 1.

[0079] Among them, the middle part of the working surface 1 can be a raised area, and the side of the working surface 1 can be a nearly straight area. It can be understood that both the middle part and the side are raised in the direction of the inner cavity of the crystallizer, but the side is flatter than the middle part, so that the crystallizer can prepare a casting 300 with a corner having a nearly right-angle structure. The corner of the casting 300 can be a casting 300 corresponding to the angle at the intersection of the wide copper plate 200 and the narrow copper plate 100. In the embodiment of the present application, the angle at which the wide copper plate 200 and the narrow copper plate 100 intersect is close to a right angle. It should be noted that the working surface 1 conforms to formula 1, and a smooth and continuous transition between the middle and the two side sides can be achieved. At the same time, it can also be achieved in the height and width direction of the narrow copper plate 100, the raised height and span of the middle part, and the raised height and width of the side are all continuous curved surface changes. The span of the middle part can be the width of the middle part.

[0080] Among them, in the embodiment of the present application, in the height direction of the narrow copper plate 100, the span of the middle raised area of ​​the working surface 1 gradually decreases from the top surface 2 to the bottom surface, that is, the lateral span of the middle raised area gradually decreases from the top surface 2 to the bottom surface.

[0081] Among them, in the embodiment of the present application, the taper compensation correction value B3 of the working surface 1 in the height direction of the narrow copper plate 100 is 0 when it is at or above the height 2y0 from the top surface of the narrow copper plate 100, and gradually increases when it is below the height 2y0 from the top surface of the narrow copper plate 100. It should be noted that in the height direction of the narrow copper plate 100, the raised height of the middle and upper area of ​​the working surface 1 is greater than the raised height of the middle and lower area of ​​the working surface 1.

[0082] Among them, in the embodiment of the present application, the working surface 1 is divided into a first convex surface 11 and a second convex surface 12 by the transverse center line 3 of the narrow copper plate. The first convex surface 11 is close to the inner arc side of the ingot 300, and the second convex surface 12 is close to the outer arc side of the ingot 300.

[0083] Among them, the area where the first convex surface 11 and the second convex surface 12 are close to the transverse center line 3 of the narrow copper plate is the middle of the working surface 1, and the area where the first convex surface 11 and the second convex surface 12 are away from the transverse center line 3 of the narrow copper plate is the edge of the working surface 1.

[0084] The working surface 1 of the narrow copper plate 100 is an asymmetric structure.

[0085] Specifically, the convex height of the first convex surface 11 gradually decreases in the direction away from the transverse center line 3 of the narrow copper plate, and the convex height of the second convex surface 12 also gradually decreases in the direction away from the transverse center line 3 of the narrow copper plate. In the embodiment of the present application, the convex height reduction rate of the first convex surface 11 is less than the convex height reduction rate of the second convex surface 12, and the convex height of the area outside the transverse center line 3 of the narrow copper plate on the first convex surface 11 is greater than the convex height of the area outside the transverse center line 3 of the narrow copper plate on the second convex surface 12, that is, the convex height of the first convex surface 11 is greater than the convex height of the second convex surface 12, so that the inner arc of the ingot 300 produced by the crystallizer prepared by the above-mentioned narrow copper plate 100 is narrow and the outer arc is wide, ensuring that the widths of the inner and outer arcs of the ingot 300 are equivalent after passing through the straightening zone, further reducing the amount of edge resection of the steel plate, and improving the yield rate of wide and thick plates.

[0086] In some possible implementations provided in this application, see Figure 3 As shown, the edge of the first convex surface 11 away from the second convex surface 12 is the first contour line 111, and the edge of the second convex surface 12 away from the first convex surface 11 is the second contour line 121. At the same height, the difference between the protrusion height of the first contour line 111 and the protrusion height of the second contour line 121 is Δh, 3mm≤Δh≤20mm.

[0087] The first contour line 111 and the second contour line 121 are both curves.

[0088] For example, the difference ⊿h between the distance between the first contour line 111 and the first plane and the distance between the second contour line 121 and the first plane can be 3mm, or 4mm, or 5mm, or 6mm, or 7mm, or 8mm, or 9mm, or 10mm, or 11mm, or 12mm, or 13mm, or 14mm, or 15mm, or 16mm, or 17mm, or 18mm, or 19mm, or 20mm. It can be understood that ⊿h can also be other values ​​besides the above values, as long as the range of ⊿h is 3 to 20mm.

[0089] Specifically, in the embodiment of the present application, at the first height, the distance between the first contour line 111 and the first plane is greater than the distance between the second contour line 121 and the first plane. The first height can be any height in the height direction of the narrow copper plate 100, and the first plane can be a vertical plane of the narrow copper plate 100 that is away from the casting 300 and parallel to the cooling surface of the narrow copper plate 100. In the embodiment of the present application, the first plane is the cooling surface. The cooling surface of the narrow copper plate 100 can be the wall surface of the narrow copper plate 100 that is away from the casting 300, and the cooling surface is a plane. For example, the distance between the intersection of the first contour line 111 and the top surface 2 of the narrow copper plate 100 and the cooling surface of the narrow copper plate 100 is greater than the distance between the intersection of the second contour line 121 and the top surface 2 of the narrow copper plate 100 and the cooling surface of the narrow copper plate 100. Similarly, the distance between the intersection of the cross section at any height below the top surface 2 of the narrow copper plate 100 and the first contour line 111 and the cooling surface of the narrow copper plate 100 is greater than the distance between the intersection of the second contour line 121 and the cooling surface of the narrow copper plate 100. In other words, the thickness of the narrow copper plate 100 on the side where the first contour line 111 is located is greater than the thickness on the side where the second contour line 121 is located.

[0090] The narrow copper plate 100 provided in the embodiment of the present application is configured such that the distance between the first contour line 111 of the edge of the first convex surface 11 and the first plane is greater than the distance between the second contour line 121 of the edge of the second convex surface 12 and the first plane, so that the thickness of the side where the first contour line 111 of the narrow copper plate 100 is located is greater than the thickness of the side where the second contour line 121 is located, so that the inner arc of the ingot 300 produced by the crystallizer using the above-mentioned narrow copper plate 100 is narrow and the outer arc is wide, thereby ensuring that the difference in the inner and outer arc widths of the ingot 300 after passing through the straightening zone is less than 3 mm, thereby reducing the defect cutting of the edge of the wide and thick plate. The purpose of removing the amount is to improve the yield rate and production efficiency of wide and thick plates; at the same time, by setting the convexity of the working surface 1 on the narrow copper plate 100 to transition continuously and smoothly from the middle to the edge, it is avoided that an additional transition zone is required for the transition between the middle and the edge of the working surface 1, and the middle width occupied by the straight area of ​​the edge is reduced, thereby solving the problem that the span of the middle convexity is too small due to the additional introduction of the transition zone, thereby failing to effectively reduce the formation of significant width edge line crack defects and significant double-strand shape defects in the billet 300 during the rolling process, and can also avoid the problem that if a smooth transition zone is not introduced between the middle and the edge of the working surface 1, The problem of leakage of the solidified billet shell is solved, which ensures that the crystallizer can prepare the ingot 300 with a narrow face, a large arc surface, a large inner concave amount, and a nearly right-angle structure at the corner with high quality, thereby significantly reducing the width of the wide side line cracks in the wide and thick plate rolling, and ensuring that the ingot 300 is straightened at high temperature at the corner in the second cooling zone, effectively preventing the occurrence of cracks at the corner of the ingot 300; at the same time, an adjustment factor is introduced into the middle convex surface span of the working surface 1 of the narrow copper plate 100, which realizes the adjustment of the middle convex span and the width of the nearly straight area of ​​the edge with the downward solidification shrinkage characteristics of the ingot 300, thereby ensuring the solidification of the inner concave surface of the ingot 300 throughout the whole process The narrow copper plate 100 is highly fitted and solidified in the horizontal direction, and the ingot 300 is efficiently and evenly solidified, while the wear on both sides of the raised arc surface in the middle of the copper plate is reduced, thereby improving the service life of the crystallizer; at the same time, the working surface 1 of the narrow copper plate 100 is a curved taper compensation structure along its height direction to cater to the solidification shrinkage characteristics of the ingot shell, which meets the characteristics of dynamic solidification of the ingot 300 in the height direction, ensuring that the narrow surface of the ingot is well fitted with the copper plate during the entire solidification process, so that the heat transfer between the two is uniform; in addition, the compensation correction value considering wear is introduced into the nearly straight edge area of ​​the working surface 1 of the narrow copper plate 100, see Figure 4 and Figure 5 As shown, the taper compensation value of the nearly straight area of ​​the edge below 312 mm from the top surface 2 gradually decreases, solving the problem of severe wear of the edge in the lower area of ​​the crystallizer in the actual continuous casting process.

[0091] In some possible implementations provided in this application, see Figure 3 As shown, at the height of the top surface 2 of the narrow copper plate 100, the difference between the raised height of the transverse center line 3 of the narrow copper plate and the raised height of the first contour line 111 is B1, 5mm≤B1≤20mm.

[0092] Among them, at the height of the top surface 2 of the narrow copper plate 100, the convex height of the transverse center line 3 of the narrow copper plate is greater than the convex height of the first contour line 111, so that the crystallizer using the above narrow copper plate 100 can prepare a narrow-surface, large-arc, and large-indent casting 300. It can be understood that the transverse center line 3 of the narrow copper plate can be the center line of the width direction of the working surface 1.

[0093] Specifically, at the height of the top surface 2 of the narrow copper plate 100, the difference between the raised height of the horizontal center line 3 of the narrow copper plate and the raised height of the first contour line 111 is B1, 5mm≤B1≤20mm. For example, at the height of the top surface 2 of the narrow copper plate 100, the difference between the raised height of the horizontal center line 3 of the narrow copper plate and the raised height of the first contour line 111 is B1, which can be 5mm, or 6mm, or 7mm, or 8mm, or 9mm, or 10mm, or 11mm, or 12mm, or 13mm, or 14mm, or 15mm, or 16mm, or 17mm, or 18mm. It can be understood that B1 can also be other values ​​besides the above values, as long as the range of B1 is 5 to 20mm.

[0094] In some possible implementations provided in this application, see Figure 2 As shown, in the height direction of the narrow copper plate 100, the width of the narrow copper plate 100 decreases linearly by 1 to 3 mm from the top surface 2 to the bottom surface. It should be noted that in the actual process of slab continuous casting, the ingot 300 solidifies in the crystallizer, and the thickness direction of the ingot 300 will shrink by 1 to 3 mm. In the present application, by setting the width of the narrow copper plate 100 to decrease linearly by 1 to 3 mm from the top surface 2 to the bottom surface, it is possible to prevent the ingot 300 from detaching from the wide copper plate 200 due to shrinkage in the thickness direction during the downward solidification process.

[0095] The structure of the narrow copper plate 100 is further described below in conjunction with specific numerical values ​​and drawings.

[0096] Among them, see Figure 1 As shown, the working surface 1 includes a first convex surface 11 and a second convex surface 12, which can be used to make a narrow copper plate 100 with an inner and outer arc asymmetric convex curved surface crystallizer. The height of the narrow copper plate 100 is 900mm, and the working surface 1 of the narrow copper plate 100 is an asymmetric structure with a wide top and a narrow bottom.

[0097] Specifically, the working surface 1 decreases linearly by 1 to 3 mm from the top surface 2 to the bottom surface in the height direction. It should be noted that, in the actual process of slab continuous casting, the ingot 300 solidifies in the crystallizer, and the thickness direction of the ingot 300 will shrink by 1 to 3 mm. In the present application, by setting the width of the working surface 1 to decrease linearly by 1 to 3 mm from the top surface 2 to the bottom surface, it is possible to prevent the ingot 300 from detaching from the wide copper plate 200 of the crystallizer due to shrinkage in the thickness direction during the downward solidification process.

[0098] Among them, in the above embodiment, the width of the working surface 1 decreases linearly by 2 mm from the top surface 2 to the bottom surface, the width of the top surface 2 of the narrow copper plate 100 is 266 mm, and the width of the bottom surface of the narrow copper plate 100 is 264 mm.

[0099] Specifically, at the height of the top surface 2 of the narrow copper plate 100, the raised height of the center line of the working surface 1 in the width direction is greater than the raised height of the first contour line 111, and the difference between the raised height of the center line of the working surface 1 in the width direction and the raised height of the first contour line 111 is B1, 5mm≤h2≤20mm.

[0100] In the above embodiment, at the height of the top surface 2 of the narrow copper plate 100, the difference B1 between the raised height of the center line of the working surface 1 in the width direction and the raised height of the first contour line 111 is 14 mm.

[0101] Specifically, at the same height, the protrusion height of the first contour line 111 is greater than the protrusion height of the second contour line 121 , and the difference between the protrusion height of the first contour line 111 and the protrusion height of the second contour line 121 is ⊿h, 3mm≤⊿h≤20mm.

[0102] In the above embodiment, at the same height, the difference Δh between the protrusion height of the first contour line 111 and the protrusion height of the second contour line 121 is 8 mm.

[0103] Among them, in the above embodiment, the working surface 1 includes a first convex surface 11 and a second convex surface 12, the central convex area of ​​the working surface 1 is the area where the first convex surface 11 and the second convex surface 12 are close to the transverse center line 3 of the narrow copper plate, and the nearly straight areas on both sides of the edge of the central convex area are the areas where the first convex surface 11 and the second convex surface 12 are away from the transverse center line 3 of the narrow copper plate, respectively. In the height and width direction of the narrow copper plate 100, the convex height and span of the central convex area, and the convex height and width of the edge are all continuous curved surface changes, and the middle and the edge are integrated and smoothly transitioned. It should be noted that the first convex surface 11 and the second convex surface 12 are smoothly transitioned and connected.

[0104] Among them, in the height direction of the narrow copper plate 100, the taper compensation value of the working surface 1 is determined according to the following method: first, the shrinkage of the corner of the ingot 300 along the width direction is calculated, and then the curve expression of the taper compensation value of the height below the meniscus of the narrow copper plate 100 is obtained by fitting a seventh-order polynomial, with the meniscus as the coordinate origin, the height of the narrow copper plate 100 and the compensation value as the horizontal and vertical coordinates respectively. On this basis, the fitted expression curve is further rotated clockwise with the bottom surface of the narrow copper plate 100 as the origin until the curve at the top surface 2 of the narrow copper plate 100 intersects with the horizontal axis, and the origin of the coordinate system is translated to the intersection, thereby obtaining the taper compensation value expression 2 of the working surface 1 of the narrow copper plate 100 from the top surface 2 to the bottom surface.

[0105] Among them, in the above embodiment, the steel type produced is AH36 steel, and its meniscus is located at a height of 100mm below the top surface 2 of the narrow copper plate 100. The shrinkage of the corner of the ingot 300 along the width direction in the meniscus and in each height direction below it is calculated, and then the seventh-order polynomial fitting coefficients shown in Formula 2 are obtained by rotating the expression curve and translating the coordinate system: A0=0; A1=0.01677; A2=-2.805E-05; A3=-4.687E-08; A4=2.114E-10; A5=-3.114E-13; A6=2.206E-16, A7=-6.320E-20. That is, the expression of Formula 2 is:

[0106] D1=0.01677y-2.805E-05y 2 -4.687E-08y 3 +2.114E-10y 4 -3.114E-13y 5 +2.206E-16y 6 -6.320E-20y 7 (6)

[0107] According to Formula 6, the maximum value of the taper compensation of the working surface 1 in the height direction is 2.35 mm, which is located 312 mm below the top surface 2 of the narrow copper plate 100, that is, y0 is 312 mm. The taper compensation values ​​of the working surface 1 at different heights of the narrow copper plate 100 are determined, as shown in Table 1.

[0108] Table 1

[0109] Distance from top surface of narrow copper plate Taper compensation value Distance from top surface of narrow copper plate Taper compensation value 0 0.00 450 2.11 30 0.48 480 2.02 60 0.90 510 1.91 90 1.26 540 1.79 120 1.56 570 1.67 150 1.81 600 1.54 180 2.01 630 1.41 210 2.15 660 1.27 240 2.25 690 1.13 270 2.32 720 0.98 300 2.34 750 0.83 312 2.35 780 0.68 330 2.34 810 0.52 360 2.31 840 0.36 390 2.26 870 0.19 420 2.20 900 0.00

[0110] Further, in the above embodiment, according to the maximum protrusion height 14 mm of the working surface 1 of the narrow copper plate 100 and the taper compensation correction value in the height direction, the lateral morphology of the working surface 1 of the narrow copper plate 100 is designed to be the curve shown in Formula 7. Wherein, the expressions of B3 and B4 are shown in Formulas 8 and 9.

[0111]

[0112] The morphology of the working surface 1 of the narrow copper plate 100 in the width direction is combined and the convex curve expression 7 in the width direction of the working surface 1 in the embodiment of the present application is determined by superposition. Figure 2 As shown. Figure 2 It can be seen that due to the introduction of the span adjustment factor in the middle convex surface of the working surface 1, the span of the middle convex area and the width of the nearly straight area at the edge gradually decrease towards the transverse center line 3 of the narrow copper plate as the distance from the top surface 2 of the narrow copper plate 100 increases, ensuring that the concave surface of the ingot 300 in the asymmetric convex curved crystallizer is highly fitted with the working surface 1 in its width direction during the solidification process and solidifies evenly, avoiding the phenomenon of the ingot 300 shrinking and locking or detaching from the working surface 1, and ensuring the long service life of the crystallizer. Figure 3 It can be seen that, due to the introduction of the height difference of the protrusions of the first contour line 111 and the second contour line 121 and the presence of nearly straight areas on both sides of the working surface 1, the narrow copper plate 100 with the working surface 1 can be used to prepare the narrow surface with a narrow inner arc side, a wide outer arc side, a concave large arc surface, and a nearly right-angled corner structure. At the same time, in the embodiment of the present application, due to the introduction of the taper compensation correction value in the nearly straight area of ​​the edge of the working surface 1, the taper compensation value of the nearly straight area of ​​the two sides of the edge below 312mm below the top surface 2 of the narrow copper plate 100 is gradually reduced, see Figure 4 and Figure 5 shown.

[0113] In the second aspect of the embodiment of the present application, see Figure 6 and Figure 7 As shown, a method for designing a working surface 1 of a narrow copper plate 100 is provided, which is used to design the working surface 1 of a narrow copper plate 100 of an asymmetric convex curved crystallizer of any one of the above items, and the method comprises:

[0114] Step 1: Use JMatPro software to calculate the high-temperature thermal / mechanical physical properties of AH36 steel; consult the standard manual to obtain the thermal physical properties of the crystallizer copper plate and cooling water, and finally import all physical property parameter relationship curves into the corresponding commercial software material database.

[0115] Specifically, referring to the actual AH36 steel composition shown in Table 2, the thermal conductivity, density, elastic modulus, enthalpy, Poisson's ratio, yield limit, linear thermal expansion coefficient, and the liquidus temperature of 1798.15K and the solidus temperature of 1738.15K at high temperature were calculated using JMatPro software. On this basis, the thermal conductivity, specific heat and density physical properties of the mold copper plate and cooling water were obtained by consulting the standard tool manual as shown in Table 3. The relationship curves between the physical properties of each material and the temperature were respectively imported into the material database of the corresponding commercial software for calculation.

[0116] Table 2

[0117] element C Si Mn P S Nb Ti Al content 0.14 1.3 0.014 0.023 0.014 0.027 0.017 0.024

[0118] Table 3

[0119]

[0120] Step 2: Direct fluid-solid coupling algorithm is used to access ANSYS Fluent and MSC.Marc commercial software using the multi-physics coupling interface MPCCI, and the three-dimensional thermal / mechanical finite element analysis of the ingot-crystallizer system and the copper plate-cooling water thermal / flow analysis are coupled to calculate the dynamic solidification heat transfer and deformation shrinkage behavior of the narrow plane structure ingot 300 in the crystallizer, as follows:

[0121] Step 201: According to the crystallizer copper plate drawing and the actual taper of the narrow surface, a three-dimensional solid model of the crystallizer consisting of two planar wide copper plates 200 and two planar narrow copper plates 100, the ingot 300 and the cooling water in the cooling water tank is created.

[0122] Specifically, according to the actual wide copper plate 200 drawing of the crystallizer, the narrow copper plate 100 drawing, and the narrow surface taper process, a three-dimensional solid model of the crystallizer consisting of two wide copper plates 200 and two narrow copper plates 100, a three-dimensional solid model of the ingot 300, and a three-dimensional solid model of cooling water in the copper plate cooling water tank are established. Among them, in the embodiment of the present application, the height of the wide copper plate 200 and the narrow copper plate of the crystallizer are both 900mm, the thickness is both 40mm, the top surface 2 of the narrow copper plate 100 is 266mm wide, the bottom surface width is 264mm, and the narrow surface taper is 1.0%.

[0123] Step 202: Import the mold copper plate, the ingot 300 and the cooling water model into ICEM-CFD for meshing, and execute different meshing strategies, while defining the contact surface between the cooling water and the copper plate as a coupling surface.

[0124] Specifically, the three-dimensional solid models of the crystallizer copper plate, the ingot 300 and the cooling water are respectively imported into the meshing software ICEM-CFD for hexahedral meshing. Among them, the mesh size of the crystallizer copper plate is 10mm, and the mesh size of the ingot 300 is 2mm; the outermost mesh of the cooling water in the water tank continues to be super dense, and the mesh size is set to 0.02mm, and the surface in contact with the copper plate in the cooling water model is defined as a coupling surface during meshing.

[0125] Step 203: Import the meshed copper plate and the ingot 300 into MSC.Marc, use unit type 7 to perform thermal / structural analysis, and assign physical property parameters to the corresponding model.

[0126] Specifically, the meshed copper plate and ingot 300 models are imported into MSC.Marc software, and the mesh units of the model are set to unit type 7 for performing thermal / structural analysis, and the physical property parameters imported into the material database in step 1 are assigned to the copper plate and ingot 300 respectively.

[0127] Step 204: According to the actual production situation of a steel plant, the position of the meniscus of the crystallizer is set and the area below the meniscus is defined as the effective height, and the downward direction of the ingot 300 is defined as the ingot drawing direction.

[0128] Specifically, based on the actual continuous casting production crystallizer liquid level height of 800mm, the meniscus position in the embodiment of the present application is defined as a height of 100mm from the upper contour line of the working surface 1 of the narrow copper plate 100, and the height below the meniscus is set as the effective height of the crystallizer, and the downward direction of the ingot 300 is defined as the billet drawing direction.

[0129] Step 205: define the cooling water tank wall surface of the copper plate model as a coupling surface for coupling calculation with the copper plate-cooling water heat / flow model.

[0130] Specifically, in the MSC.Marc software, the cooling water tank wall of the copper plate model is defined as a coupling surface for coupling calculation with the copper plate-cooling water thermal / fluid model.

[0131] Step 206: Establish a heat flow model of the shell-crystallizer interface that takes into account the dynamic changes of the interface gap between the shell and the copper plate, the protective slag film and the air gap.

[0132] Specifically, a heat flow model of the shell-crystallizer interface is established considering the interface gap between the shell and the copper plate, the dynamic changes of the protective slag film and the air gap, and the calculation of the interface heat flow is determined by solving the simultaneous equations of equations 10 to 19.

[0133]

[0134] Where q is the interface heat flux density; T shellis the surface temperature of the ingot 300, which is calculated by a three-dimensional thermal / mechanical finite element model of the ingot-crystallizer system; T mold is the hot surface temperature of the copper plate, which is also calculated by the three-dimensional thermal / mechanical finite element model of the ingot-crystallizer system; R is the comprehensive thermal resistance of the interface, which is determined by Formula 11.

[0135]

[0136] In the formula, h rad is the comprehensive radiation heat transfer coefficient, determined by formula 12; h cond is the comprehensive conduction heat transfer coefficient, determined by Eq. 13.

[0137]

[0138] In the formula, σ SB is the Stefan-Boltzmann constant; ∈ shell is the emissivity of the solidified shell; mold is the emissivity of the copper plate of the crystallizer; T melt is the melting temperature of the protective slag; R int is the thermal resistance of the crystallizer-solid slag layer interface, determined by equation 14; d liq is the thickness of the liquid protective slag layer, determined by formula 15; d sol is the thickness of the solid protective slag layer, determined by formula 16; d air is the air gap thickness, determined by equation 17; k liq k is the thermal conductivity of liquid mold slag; sol k is the thermal conductivity of solid mold slag; air is the thermal conductivity of air.

[0139] R int =(96014T melt -9604.3) 2 ×10 -11 (14)

[0140]

[0141] d gap =d liq +d sol +d air (17)

[0142] Where, d gap is the total thickness of the interface gap between the billet shell and the copper plate of the crystallizer. Based on the principle of equal heat flow through each heat transfer medium layer in the interface, according to the surface temperature T shell The melting temperature of the mold slag T melt Relationship, the above formulas can be substituted into the following equation group to solve the interface heat flux q.

[0143] q=q melt =q sol =q int (18)

[0144] or,

[0145] q=q air =q sol =q int (19)

[0146] In the formula, q melt is the heat flux density of the liquid protective slag layer; q sol is the heat flux density of the solid protective slag layer; q air is the heat flux density of the air gap layer; q int is the interface heat flux density between the solid protective slag and the copper plate of the crystallizer. The corresponding parameters in the above formulas are detailed in Table 4.

[0147] Table 4

[0148] Parameter name unit Numeric <![CDATA[Stefan-Boltzmann constant σ SB > <![CDATA[W / (m 2 ·K 4 )]]> <![CDATA[5.67×10 -8 ]]> <![CDATA[Protecting slag melting temperature, T melt > K 1463 <![CDATA[Thermal conductivity of liquid mold flux, k liq > W / (m·K) 1.8 <![CDATA[Thermal conductivity of solid mold powder, k sol > W / (m·K) 1.63 <![CDATA[Thermal conductivity of air, k air > W / (m·K) 0.047 <![CDATA[Solidified shell emissivity, ∈ shell > 0.8 <![CDATA[Emissivity of the mold copper plate, ∈ mold > 0.8

[0149] Step 207: setting the initial temperature conditions of the copper plate and the casting slab 300.

[0150] Specifically, based on the actual continuous casting of AH36 steel on site and its casting temperature, the initial temperature of the wide and narrow copper plate 100 is set to 395K, and the initial temperature of the ingot 300 is set to 1823.2K.

[0151] Step 208: According to step 216, dynamically set the heat transfer boundary conditions of the copper plate cooling water trough, the heat transfer boundary conditions between the ingot 300 and the copper plate determined by step 206, the downward displacement constraint of the ingot 300, the fixed constraint of the bolt hole, and the static pressure of the molten steel applied to the solidification front of the ingot 300.

[0152] Specifically, the temperature boundary conditions and mechanical boundary conditions of the copper plate and the ingot 300 are set. Among them, the heat transfer boundary conditions of the copper plate cooling water tank are dynamically set by the coupling interface based on the flow and heat transfer calculation results of the cooling water in step 216; the heat transfer boundary conditions between the ingot 300 and the copper plate are dynamically determined by the shell-crystallizer interface heat flow model in step 206; a downward displacement constraint equivalent to a pulling speed of 1.1m / min is applied to the ingot 300, and a completely fixed displacement constraint is set for the fastening bolt holes on the back of the copper plate. The interaction force boundary between the ingot 300 and the copper plate is set using the "rigid body-deformable body" contact pair analysis setting. The molten steel static pressure boundary condition is applied to the solidification front of the ingot 300, and the value of the molten steel static pressure is determined by formula 20.

[0153] P=ρ s (T)gh (20)

[0154] Where P is the static pressure of molten steel, Pa; ρ s (T) is the density of the ingot 300 at temperature T; g is the acceleration due to gravity, which is 9.81 m / s 2 ; h is the vertical height from the meniscus.

[0155] Step 209: Select a constitutive equation that reflects the high temperature deformation characteristics of the ingot 300.

[0156] Specifically, a constitutive equation reflecting the high temperature deformation characteristics of the ingot 300 is selected. In the embodiment of the present application, considering that creep, elastic deformation and plastic deformation occur simultaneously during the solidification process of the ingot 300, the equations shown in equations 21 to 24 are selected as the mechanical constitutive equations of the ingot 300.

[0157]

[0158] In the formula, is the equivalent strain rate; is the equivalent stress; t is the current time; C is the pre-exponential factor, which is given by Formula 22; Q is the ratio of the viscoplastic deformation activation energy to the gas constant, which is 17160K-1 in the embodiment of the present application; n and m are the exponents of stress and time, respectively, which are given by Formula 23 and Formula 24, respectively.

[0159] C=0.3091+0.209w c +0.1773w c 2 (twenty two)

[0160] In the formula, w c is the mass fraction of carbon in AH36 steel, see Table 3.

[0161] n=6.365-4.521×10 -3 T shell +1.439×10 -6 T shell 2 (twenty three)

[0162] m=-1.362+5.761×10 -4 T shell +1.982×10 -8 T shell 2 (twenty four)

[0163] Step 210: Set the analysis type between the ingot 300 and the crystallizer to transient thermal / structural analysis.

[0164] Step 211: Determine the model calculation time and time step based on the actual production pulling speed and the effective height of the crystallizer.

[0165] Specifically, based on the actual pulling speed of 1.1 m / min of AH36 steel produced by a steel plant, the calculation time of the model is determined to be 43.64 s, and the time step is set to 0.01 s.

[0166] Step 212: Using the unit birth and death function, set the participation status of the ingot 300 unit in the transient thermal / structural calculation of the crystallizer copper plate.

[0167] Specifically, the unit life and death function of the Marc software is used to set whether the slab 300 unit participates in the transient thermal / structural calculation between it and the copper plate of the crystallizer according to whether the slab 300 unit is located in the effective height area below the meniscus of the crystallizer. If the slab 300 unit is located at or below the meniscus of the crystallizer, the transient thermal / structural calculation of the slab 300 and the copper plate of the crystallizer is performed; otherwise, the slab 300 unit is frozen so that it does not participate in the transient thermal / structural calculation of the two.

[0168] Step 213: Import the cooling water model mesh into Fluent, turn on the energy equation option and select the k-epsilon turbulence model.

[0169] Step 214: Set the physical parameters of the cooling water and the water tank wall, set the cooling water inlet velocity, initial temperature, initial temperature of the coupling surface, turbulent kinetic energy and turbulent dissipation rate.

[0170] Specifically, the physical properties of the cooling water and copper plate imported into the material database in step 1 are assigned to the cooling water and the water tank wall respectively, and the cooling water inlet velocity, cooling water temperature, initial contact temperature of the coupling surface, and turbulent kinetic energy are set to 7.5 m / s, 305 K, 305 K, and 0.3528 m 2 / s 2 and turbulent dissipation rate 1115.087m 2 / s 3 .

[0171] Step 215: The thermal / mechanical model of the ingot-crystallizer copper plate and the thermal / flow model of the copper plate-cooling water are coupled through the MPCCI interface.

[0172] Specifically, the thermal / mechanical coupling finite element model of the ingot-crystallizer copper plate system and the thermal / fluid coupling calculation model of the copper plate-cooling water system are connected to the coupling calculation interface MPCCI.

[0173] Step 216: The thermal / mechanical model of the ingot-crystallizer copper plate and the thermal / flow model of the copper plate-cooling water are coupled through the MPCCI interface to achieve a two-way exchange of heat flux density and temperature data to update the respective heat transfer boundary conditions.

[0174] Specifically, the heat flux density calculated by the thermal / fluid coupling calculation model of the copper plate-cooling water system is applied to the thermal / mechanical coupling finite element model of the ingot-crystallizer copper plate system as the heat transfer boundary condition of the copper plate cooling water trough wall. At the same time, the thermal / mechanical coupling finite element model of the ingot-crystallizer copper plate system returns the calculated temperature and heat flux density to the thermal / fluid coupling calculation model of the copper plate-cooling water system, and updates the heat transfer boundary condition of the cooling water in the thermal / fluid coupling calculation model of the copper plate-cooling water system.

[0175] Step 217: Set parallel computing.

[0176] Specifically, parallel calculation is set, and model calculation is executed until the calculation is completed, and the solidification shrinkage of the corners of the narrow plane structure ingot 300 at various heights below the meniscus of the crystallizer along the wide surface direction is extracted.

[0177] Step 3: Using the result of step 217, determine the shrinkage of the ingot 300 at each height below the meniscus of the crystallizer through polynomial fitting, and then determine the curve expression D1 of the taper compensation value of the working surface 1. Specifically, according to step 217, the shrinkage of the corner of the narrow plane structure ingot 300 at each height below the meniscus of the crystallizer is calculated along the width center direction, and the height of the narrow copper plate 100 and the compensation value are used as the horizontal and vertical coordinates, respectively, and the height of the meniscus is used as the origin of the coordinate system. The curve expression of the taper compensation value of the working surface 1 of the narrow copper plate 100 at the height below the meniscus is obtained through seventh-order polynomial fitting. On this basis, further use the curve at the height of the lower mouth contour line of the working surface 1 of the narrow copper plate 100 as the origin, rotate the curve clockwise until the curve at the upper mouth contour line of the working surface 1 of the narrow copper plate 100 intersects with the horizontal axis, and translate the origin of the coordinate system to the intersection, and then perform seventh-order polynomial fitting according to the function of formula 2 to obtain each coefficient A i value, establish the D1 expression.

[0178] Step 4: Based on the height and width of the narrow copper plate 100 , determine the convex curve expression D2 of the working surface 1 in the width direction of the narrow copper plate 100 .

[0179] Step 5: Add the expression for determining the taper compensation value of working surface 1 to the expression for the convex curve in the width direction of working surface 1 to complete the design of expression D of working surface 1.

[0180] In the third aspect of the embodiment of the present application, see Figure 8 As shown, a crystallizer is provided, comprising any one of the narrow copper plates 100 described above, wherein two narrow copper plates 100 are arranged opposite to each other, and the crystallizer further comprises two oppositely arranged wide copper plates 200, wherein the combination of the two oppositely arranged wide copper plates 200 and the two oppositely arranged narrow copper plates 100 is suitable for forming an inner cavity for solidifying molten steel into a casting billet 300.

[0181] The embodiment of the present application provides a narrow copper plate 100, a design method for a working surface 1 of the narrow copper plate 100, and a crystallizer, wherein the narrow copper plate 100 sets the distance between the first contour line 111 of the edge of the first convex surface 11 and the first plane to be greater than the distance between the second contour line 121 of the edge of the second convex surface 12 and the first plane, so that the thickness of the side where the first contour line 111 of the narrow copper plate 100 is located is greater than the thickness of the side where the second contour line 121 is located, so that the inner arc of the ingot 300 produced by the crystallizer using the above-mentioned narrow copper plate 100 is narrow and the outer arc is wide, thereby ensuring that the ingot 300 is straightened after the straightening process. The rear portion is rectangular, so as to achieve the purpose of reducing the amount of defect removal at the edge of the wide and thick plate, thereby improving the yield rate and production efficiency of the wide and thick plate; at the same time, by setting the convexity of the working surface 1 on the narrow copper plate 100 to transition continuously and smoothly from the middle to the edge, it is avoided that an additional transition zone is required for the transition between the middle and the edge of the working surface 1, and the width occupied by the straight area of ​​the edge is reduced, thereby solving the problem that the span of the middle convexity is too small due to the additional introduction of the transition zone, thereby failing to effectively reduce the formation of significant width edge line crack defects and significant double-strand shape defects of the ingot 300 during the rolling process, and also avoiding the transition between the middle and the edge of the working surface 1. The problem of leakage of the solidified billet shell caused by the lack of a smooth transition zone is solved, which ensures that the crystallizer can prepare the ingot 300 with a narrow face, a large arc surface, a large inner concave amount, and a nearly right-angle structure at the corner with high quality, thereby significantly reducing the width of the wide side line cracks of the wide and thick plate rolling, and ensuring that the ingot 300 is straightened at high temperature at the corner in the second cooling zone, effectively preventing the generation of cracks at the corner of the ingot 300; at the same time, an adjustment factor is introduced into the middle convex surface span of the working surface 1 of the narrow copper plate 100, so that the middle convex span and the width of the nearly straight zone at the edge are adjusted along with the downward solidification shrinkage characteristics of the ingot 300, thereby ensuring the inner concave of the ingot 300 During the whole solidification process, the narrow copper plate 100 is highly fitted and solidified in the horizontal direction. While the ingot 300 is efficiently and evenly solidified, the wear on both sides of the raised arc surface in the middle of the copper plate is reduced, thereby improving the service life of the crystallizer. At the same time, the working surface 1 of the narrow copper plate 100 is a curved taper compensation structure along its height direction to cater to the solidification shrinkage characteristics of the ingot shell, which meets the characteristics of dynamic solidification of the ingot 300 in the height direction, ensuring that the narrow surface of the ingot is well fitted with the copper plate during the whole solidification process, so that the heat transfer between the two is uniform. In addition, the compensation correction value considering wear is introduced into the nearly straight edge area of ​​the working surface 1 of the narrow copper plate 100, see Figure 4 and Figure 5 As shown, the taper compensation value of the nearly straight area of ​​the edge below 312 mm from the top surface 2 gradually decreases, solving the problem of severe wear of the edge in the lower area of ​​the crystallizer in the actual continuous casting process.

[0182] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed.

[0183] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above are only preferred implementations of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. A narrow copper plate, characterized in that: Applied to a crystallizer, the crystallizer has an inner cavity for solidifying molten steel into a cast billet, and the narrow copper plate includes a working surface, which is a curved surface structure convex toward the inner cavity, and the working surface of the curved surface structure conforms to the formula: D=DD1+D,2 Wherein, D1 is the expression of the taper compensation value of the working surface in the height direction of the narrow copper plate; D2 is the expression of the convex curve of the working surface in the width direction of the narrow copper plate; Among them, the working surface includes a first convex surface and a second convex surface. The first convex surface is arranged on one side of the transverse center line of the narrow copper plate, and the second convex surface is arranged on the other side of the transverse center line of the narrow copper plate. The protrusion heights of the first convex surface and the second convex surface gradually decrease in the direction away from the transverse center line of the narrow copper plate, and the slope of the first convex surface is smaller than the slope of the second convex surface.

2. The narrow copper plate according to claim 1, characterized in that: The edge of the first convex surface away from the second convex surface is the first contour line, and the edge of the second convex surface away from the first convex surface is the second contour line. At the same height, the difference between the convex height of the first contour line and the convex height of the second contour line is Δh, 3mm≤Δh≤20mm.

3. The narrow copper plate according to claim 1, characterized in that: At the height of the top surface of the narrow copper plate, the difference between the raised height of the transverse center line of the narrow copper plate and the raised height of the first contour line is B1, 5mm≤B1≤20mm.

4. The narrow copper plate according to claim 1, characterized in that: The taper compensation value expression of the working surface in the height direction of the narrow copper plate conforms to the formula: In the formula, A i is the fitting coefficient of the seventh-order polynomial; y is the distance from the top surface of the narrow copper plate.

5. The narrow copper plate according to claim 3, characterized in that: The convex curve expression of the working surface in the width direction of the narrow copper plate conforms to the formula: In the formula, x is the position relative to the transverse center line of the narrow copper plate in the width direction of the narrow copper plate. When x is a negative value, it is located on the first convex surface, and when x is a positive value, it is located on the second convex surface; B2 is the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate; B3 is the taper compensation correction value of the working surface of the narrow copper plate in the height direction.

6. The narrow copper plate according to claim 5, characterized in that: The adjustment factor of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate conforms to the formula: Where l1 is the height of the narrow copper plate.

7. The narrow copper plate according to claim 5, characterized in that: The taper compensation correction value of the working surface of the narrow copper plate in the height direction conforms to the formula: Where l2 is the width of the top surface of the narrow copper plate; y0 is the y value when D1 takes the maximum value.

8. The narrow copper plate according to claim 1, characterized in that: In the height direction of the narrow copper plate, the width of the narrow copper plate decreases linearly by 1 to 3 mm from the top surface to the bottom surface.

9. A method for designing a working surface of a narrow copper plate, characterized in that: The method for designing a working surface of a narrow copper plate according to any one of claims 1 to 8 comprises: Step 1: Obtain high temperature thermal / mechanical properties of steel and thermal properties of the mold copper plate and cooling water; Step 2: Using the direct fluid-solid coupling algorithm, calculate the solidification shrinkage of the ingot from the corner to the center of the wide surface in the crystallizer with the working surface of the narrow copper plate as a plane structure; Step 3: Based on the distribution of the solidification shrinkage from the corner of the ingot to the center of the wide surface of the crystallizer in the height direction of the crystallizer, determine the expression of the taper compensation value of the working surface in the height direction of the narrow copper plate; Step 4: Based on the height and width of the narrow copper plate, determine the convex curve expression of the working surface in the width direction of the narrow copper plate; Step 5: Based on the expression of the taper compensation value of the working surface in the height direction of the narrow copper plate and the expression of the convex curve of the working surface in the width direction of the narrow copper plate, determine the surface expression of the working surface.

10. A crystallizer, characterized in that: The invention comprises a narrow copper plate according to any one of claims 1 to 8, wherein two narrow copper plates are arranged opposite to each other, and the crystallizer further comprises two wide copper plates arranged opposite to each other, and the combination of the two wide copper plates arranged opposite to each other and the two narrow copper plates arranged opposite to each other is suitable for forming an inner cavity for solidifying molten steel into a casting billet.