Variable-focus ultrasonic-TIG (Tungsten Inert Gas) coaxial composite welding device and welding method
By using split buoy rods and ceramic insulating rings in the TIG welding device, the magnification and focal length of ultrasonic energy are adjusted, and combined with air guide holes and water-cooled tanks to achieve heat dissipation, the thermal cracks and heat dissipation of TIG welding nickel-based 690 alloy are solved. Problem: Adapt to different joint forms and improve welding stability and quality.
Patent Information
- Application Number
- CN202411369838.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
When TIG welded nickel-based 690 alloy, there are high thermal crack sensitivity, large molten pool viscosity, poor thermal conductivity, and coarse weld grain structure. In addition, there are poor heat dissipation of ultrasonic arc coaxial composite devices, easy to damage transducers, and concave spherical changes. The focal length of the sieve rod is fixed and cannot adapt to various joint forms and parts coaxial requirements.
A variable-zoom ultrasonic-TIG coaxial composite welding device is designed, using a split-type buoy rod and a ceramic insulating ring. By adjusting the diameter and radius of curvature of the buoy rod, it changes the magnification and focal length of the ultrasonic energy, combined with the air guide hole and The annular water-cooled tank achieves effective heat dissipation and forms a uniform gas laminar flow through the annular gas nozzle to protect the arc.
Effectively control welding temperature, improve welding stability and welding quality, adapt to different joint forms, extend the service life of the device, and obtain high-performance welded joints.
Smart Images

Figure CN118989688A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding, and in particular relates to a variable-focus ultrasonic-TIG coaxial composite welding device and a welding method. Background Art
[0002] As a clean energy with sustainable supply, nuclear power has become an important part of my country's energy. With the rapid development of nuclear power in my country, 690 nickel-based alloy welding materials are widely used in nuclear power equipment as a new type of corrosion-resistant and stress corrosion cracking-resistant welding materials. In the production of nuclear power, TIG welding is often used for the elbows and straight pipes of U-shaped heat transfer tubes. TIG welding is a common welding method. It is a welding method that uses an infusible tungsten electrode to generate an arc under the protection of an inert gas to heat and melt the workpiece; TIG welding has the advantages of high welding quality, high welding efficiency, and high welding flexibility. However, when TIG welding is used to weld nickel-based 690 alloy, there is a problem of high sensitivity to thermal cracks, especially high-temperature low-plasticity cracks (DDC); tiny high-temperature deplasticity cracks are easily used as crack sources and expand into macro cracks, causing the welded joint to fail, which poses a major hidden danger to the safe and reliable operation of nuclear equipment.
[0003] Some studies have proposed that introducing ultrasonic energy into TIG welding can increase the depth of the molten pool, refine the structure, and obtain high-performance welding joints. At present, there are several mainstream ultrasonic-assisted TIG welding methods. The first method is to apply ultrasound to the welding wire, and transfer ultrasonic energy into the molten pool through the welding wire as a medium; the second method is to apply ultrasonic vibration to the workbench or directly to the base material, so that the ultrasonic energy is transferred into the molten pool; the third method is arc ultrasound, which modulates the arc through high-frequency current and excites the arc to generate ultrasonic waves, thereby introducing ultrasonic energy into the molten pool through the arc; the fourth method is coaxial compounding of ultrasound and arc, which acts on the molten pool while changing the arc shape and droplet transition by emitting ultrasonic energy through the ultrasonic transmitting end. Among them, the ultrasonic arc coaxial compound equipment is simple to manufacture, has few restrictions, is easy to adjust and maintain, and has obvious effects, which has great advantages over other methods. However, the current ultrasonic arc compound device has serious heat generation, easy to burn the transducer during long-term operation, fixed focal length of the concave spherical amplitude rod, cannot adapt to various joint forms, and has high coaxiality requirements for parts in various parts.
[0004] Therefore, a new type of welding device is urgently needed to solve the problems of severe heating, fixed focal length of concave spherical amplitude transformer, inability to adapt to various joint forms, and high coaxiality requirements for parts in various parts. Summary of the invention
[0005] In view of the above-mentioned technical problems, the present invention proposes a variable-focus ultrasonic-TIG coaxial composite welding device and welding method. The invention solves the problems of high viscosity of the molten pool, poor thermal conductivity, coarse grain structure of the weld, high sensitivity to thermal cracks, etc. faced by traditional TIG welding in the process of welding nickel-based 690 alloy, and improves the problems of poor heat dissipation of the existing ultrasonic arc coaxial composite device, easy accumulation of high temperature inside the device, easy damage to the transducer and ultrasonic power supply under long-term operation, fixed ultrasonic energy amplification factor, and single focal length of the concave spherical horn.
[0006] In order to solve the above problems, the following technical solutions are adopted.
[0007] A variable-focus ultrasonic-TIG coaxial composite welding device comprises a TIG welding system; an ultrasonic vibration system is mounted on the TIG welding system; the ultrasonic vibration system is fixedly connected to one end of a lower cover 5; and the other end of the lower cover 5 is fixedly connected to a nozzle 6; The TIG welding system comprises a copper rod 1; one end of the copper rod 1 is threadedly connected to an upper cover 7; an air guide hole 12 is provided on the upper cover 7; a tungsten electrode clamp 8 is provided at the other end of the copper rod 1; the tungsten electrode clamp 8 is connected to a tungsten electrode 11; an insulating gasket 9 is provided on the tungsten electrode clamp 8 near the copper rod 1; a circular gas nozzle 10 is provided on the tungsten electrode clamp 8 near the insulating gasket 9; the circular gas nozzle 10 does not contact the tungsten electrode clamp 8, and is fixedly connected to the lower cover 5 by interference fit; The ultrasonic vibration system includes an upper cover 2, which is fixedly connected to the transducer 3; the transducer 3 is fixedly connected to the split horn 4; the upper cover 2 is fixedly connected to the upper cover 7; and holes are opened at the axis of the ultrasonic vibration system for installing a TIG welding system.
[0008] Furthermore, the split-type amplitude transformer 4 is a split-type concave spherical amplitude transformer; it includes a vibration receiving end 401 and an energy transmitting end 402, and the vibration receiving end 401 and the energy transmitting end 402 are fixedly connected by threads; the energy transmitting end 402 is a concave spherical end face; the node position of the split-type amplitude transformer 4 is provided with an insulating ring 403 and an annular water cooling groove 404.
[0009] Furthermore, fan-shaped holes are symmetrically opened on both sides of the inner wall of the insulating ring 403; and the insulating ring 403 is made of ceramic material.
[0010] Furthermore, the current circuits of the TIG welding system and the ultrasonic vibration system are independent of each other.
[0011] The welding method using the welding device comprises the following steps: Step 1: Pre-welding treatment of workpiece; Step 2: Select the horn transmitting end according to the material of the workpiece to be welded and the form of the welding joint, and adjust the nozzle height; Step 3: Turn on water cooling and air cooling, perform ordinary TIG welding and then ultrasonic welding to obtain a high-performance welded joint.
[0012] Furthermore, the step 1 is specifically as follows: before welding, the burrs, oxide layer and oil stains on the surface of the workpiece to be welded are fully cleaned, and the workpiece to be welded is fixed.
[0013] Furthermore, step 2 is specifically as follows: adjusting the position of the welding gun on the automatic walking device, selecting a variable amplitude rod transmitting end with a suitable diameter and curvature radius according to the material of the workpiece to be welded and the form of the welding joint, so that the welding area of the workpiece to be welded is at a distance from the concave end face of the variable amplitude rod to the focal length position of the sound field, and adjusting the nozzle height so that the tungsten electrode extends 4 to 6 mm outside the nozzle.
[0014] Furthermore, the step 3 is specifically as follows: adjust and determine the parameters of the welding power supply and the ultrasonic power supply, pass the welding shielding gas, open the water cooling valve and the air cooling valve, perform ordinary TIG welding, and then turn on the ultrasonic power supply for ultrasonic assisted welding to obtain a high-performance welded joint. After the welding is completed, turn off the welding power supply first, and then turn off the ultrasonic power supply.
[0015] Compared with the prior art, the present invention has the following advantages.
[0016] The present invention is designed with air guide holes and annular water cooling grooves. Cold air passes through the air guide holes and the central through hole of the TIG welding system to realize gas flow and achieve a cooling effect. Cold water passes through the annular water cooling groove to reduce the temperature increase of the split-type amplitude transformer caused by the heat radiation of the arc and the molten pool during the welding process. In this way, the temperature of the device during welding can be effectively controlled, and it is more suitable for long-term operation. An insulating ring with a fan-shaped hole is designed at the internal node position of the split-type amplitude transformer. On the one hand, it can make the argon gas pass evenly during the air cooling process and form a double airflow protection with the external protective gas nozzle of the split-type amplitude transformer. On the other hand, it can fix the tungsten electrode clamp to ensure the coaxiality of the tungsten electrode and improve the stability of welding. The design of the annular protective gas nozzle can form a uniform gas laminar flow, improve the gas protection effect, and effectively prevent the arc deviation caused by unstable airflow.
[0017] The present invention designs a split-type amplitude transformer, in which the vibration receiving end and the energy emitting end of the traditional concave spherical amplitude transformer are manufactured separately, and the two are connected by a thread, so that the energy emitting end of the amplitude transformer with different diameters and curvature radii can be matched with the vibration receiving end; the ultrasonic amplification factor can be changed by replacing the amplitude transformer emitting ends with different diameters, and the input energy can be adjusted; the focal length of the ultrasonic energy can be changed by replacing the amplitude transformer emitting ends with different curvature radii, so as to match different forms of welding joints. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1It is a schematic diagram of the assembly of the present invention.
[0019] Figure 2 Schematic diagram of TIG welding system.
[0020] Figure 3 Schematic diagram of the upper cover.
[0021] Figure 4 This is a schematic diagram of a split-type horn.
[0022] Figure 5 Schematic diagram of the vibration receiving end and the energy transmitting end.
[0023] Figure 6 It is a cross-sectional view of the concave spherical end face of the split horn.
[0024] Figure 7 Schematic diagram of the water cooling tank location.
[0025] Figure 8 Schematic diagram of the insulating ring.
[0026] Fig. 9 Metallographic diagram of the microstructure (a, Example 2 without ultrasound, 50 μm; b, Example 2 without ultrasound, 20 μm; c, Example 2 with ultrasound, 50 μm; d, Example 2 with ultrasound, 20 μm).
[0027] Among them, 1. copper rod; 2. upper cover; 3. transducer; 4. split amplitude transformer; 5. lower cover; 6. nozzle; 7. upper cover; 8. tungsten electrode clamp; 9. insulating gasket; 10. annular gas nozzle; 11. tungsten electrode; 12. air guide hole; 401. vibration receiving end; 402. energy transmitting end; 403. insulating ring; 404. annular water cooling groove. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1.
[0030] like Figure 1-Figure 3 As shown, this embodiment provides a variable-focus ultrasonic-TIG coaxial hybrid welding device, including a TIG welding system; an ultrasonic vibration system is mounted on the TIG welding system; the ultrasonic vibration system is fixedly connected to one end of a lower cover 5; and the other end of the lower cover 5 is fixedly connected to a nozzle 6; The TIG welding system comprises a copper rod 1; one end of the copper rod 1 is threadedly connected to an upper cover 7; an air guide hole 12 is provided on the upper cover 7; a tungsten electrode clamp 8 is provided at the other end of the copper rod 1; the tungsten electrode clamp 8 is connected to a tungsten electrode 11; an insulating gasket 9 is provided on the tungsten electrode clamp 8 near the copper rod 1; a circular gas nozzle 10 is provided on the tungsten electrode clamp 8 near the insulating gasket 9; the circular gas nozzle 10 does not contact the tungsten electrode clamp 8 and is fixedly connected to the lower cover 5 by interference fit. The shielding gas flows out through the circular nozzle 10, which is conducive to forming a uniform laminar flow and improving the protective effect of the gas. The circular nozzle 10 is fixed inside the lower cover 5 by interference fit. Since the acoustic focal length of the concave spherical end surface of the split horn 4 is a fixed value, in order to maximize the influence of ultrasonic waves on the molten pool, the distance between the concave spherical surface of the split horn 4 and the molten pool should be close to a fixed value. For T-joints or surfacing joints that may appear in the actual welding process, the height of the nozzle 6 can be adjusted by cooperating with the lower cover 5. Under the premise of ensuring the maximum intensity of the acoustic field acting on the molten pool, the length of the tungsten electrode extending out of the nozzle can be adjusted to meet various working conditions.
[0031] The ultrasonic vibration system includes an upper cover 2, which is fixedly connected to a transducer 3; the transducer 3 is fixedly connected to a split horn 4; the split horn 4 is a split concave spherical horn; the upper cover 2 is fixedly connected to the upper cover 7; and holes are opened at the axis of the ultrasonic vibration system for installing a TIG welding system. The ultrasonic power supply is connected to the transducer 3 through a wire to convert high-frequency current into mechanical vibration, thereby generating sound waves. The split horn 4 is tightly connected to the transducer 3 through bolts, which amplifies the mechanical vibration of the transducer 3 and concentrates the ultrasonic energy on the end face of the split horn 4, emitting ultrasonic energy to the area to be welded on the workpiece.
[0032] During welding, the synergistic effect of ultrasound and arc causes the arc to shrink, improve arc stiffness, stir the molten pool, thereby increasing the molten pool depth, refining the structure, and obtaining a high-performance welded joint.
[0033] like Figure 4-Figure 7 As shown, in this embodiment, the split-type amplitude transformer 4 includes a vibration receiving end 401 and an energy transmitting end 402, and the vibration receiving end 401 and the energy transmitting end 402 are fixedly connected by threads; the energy transmitting end 402 is a concave spherical end face; an insulating ring 403 and an annular water cooling groove 404 are provided at the node position of the split-type amplitude transformer 4.
[0034] Different from the traditional stepped horn, the vibration receiving end and the energy transmitting end of the horn are made into two independent parts, which are tightly connected by threads. Different purposes can be achieved by replacing different horn energy transmitting ends: by replacing horn energy transmitting ends of different diameters, the effect of adjusting the ultrasonic energy amplification factor can be achieved to match the optimal ultrasonic energy required for welding different materials; by replacing the concave spherical horn energy transmitting end with different curvature radii, the effect of changing the ultrasonic energy focusing focal length can be achieved to address the problem that different welding joints, such as V-shaped grooves, require different focal lengths due to different depths.
[0035] The annular water cooling groove 404 is arranged at the node position of the split horn 4, and cold water passes through the annular water cooling groove 404 to reduce the temperature increase of the horn caused by the arc and the heat radiation of the molten pool during the welding process.
[0036] like Figure 8 As shown, in this embodiment, fan-shaped holes are symmetrically opened on both sides of the inner wall of the insulating ring 403; the insulating ring 403 is made of ceramic material.
[0037] The main body of the TIG welding system is placed in the ultrasonic system. In order to prevent the copper rod 1, tungsten electrode clamp 8, tungsten electrode 11 from contacting the inner wall of the transducer 3 and the split-type amplitude transformer 4 due to vibration or other factors during the welding process, thereby causing damage to the ultrasonic system, a ceramic inner insulating ring 403 is installed at the node of the inner wall of the amplitude transformer. At the same time, the insulating ring 403 can also lock the tungsten electrode clamp 11, and fan-shaped holes are symmetrically opened on both sides of the inner wall of the insulating ring 403 to allow the circulation of argon gas after the start of air cooling.
[0038] In this embodiment, the current circuits of the TIG welding system and the ultrasonic vibration system are independent of each other.
[0039] The equipment is simple to manufacture, and the required welding power supply and ultrasonic power supply are the same as those commonly used in engineering. There is no need to customize the welding motor and ultrasonic power supply. The equipment is simple and easy to use, low in cost, and easy to debug and maintain as a whole. In situations where ultrasonic assisted welding is not required, only the TIG welding circuit can be turned on for ordinary TIG welding.
[0040] Example 2.
[0041] The welding method using the welding device comprises the following steps: Step 1. Pre-welding treatment of workpiece: before welding, clean the burrs, oxide layer and oil stains on the surface of the nickel-based 690 alloy workpiece to be welded, and fix the workpiece to be welded; Step 2, adjust the position of the welding gun on the automatic walking device, select the horn transmitting end with appropriate diameter and curvature radius according to the material welding joint form of the workpiece to be welded. In this example, nickel-based 690 alloy is selected for welding. The selected horn receiving end diameter is 50mm, the horn transmitting end diameter is 20mm, and the curvature radius is 14mm; make the distance between the welding area of the workpiece to be welded and the concave end face of the horn be the focal length position of the sound field, adjust the nozzle height, and make the tungsten electrode extend 4mm outside the nozzle; Step 3, adjust and determine the parameters of the welding power supply and the ultrasonic power supply. In this example, the welding current is selected as 100A, the welding voltage is 20V, the welding speed is 120mm / min, the ultrasonic power is 1600W, and the frequency is 20Khz; pass the welding shielding gas, open the water cooling valve and the air cooling valve, the water cooling enters from the annular water cooling groove, and the air cooling enters from the air guide hole, and perform ordinary TIG welding; then turn on the ultrasonic power supply for ultrasonic-assisted welding to obtain a high-performance welding joint. After welding, turn off the welding power supply first, and then turn off the ultrasonic power supply.
[0042] Depend on Fig. 9 Comparison of the metallographic images of (a) (b) non-ultrasonic TIG welding welds and (c) (d) ultrasonic TIG welding welds shows that when ultrasonic energy is introduced into the weld, the grain refinement effect is obvious, the grain boundary morphology is improved, and the grain boundary becomes more curved. This is because the ultrasonic energy causes cavitation and oscillation in the molten pool, which refines the grains and plays a positive role in resisting the initiation of DDC cracks.
Claims
1. A variable focus ultrasonic-TIG coaxial hybrid welding device, characterized in that: It comprises a TIG welding system; an ultrasonic vibration system is mounted on the TIG welding system; the ultrasonic vibration system is fixedly connected to one end of a lower cover (5); and the other end of the lower cover (5) is fixedly connected to a nozzle (6); The TIG welding system comprises a copper rod (1); one end of the copper rod (1) is threadedly connected to an upper cover (7); a gas guide hole (12) is provided on the upper cover (7); a tungsten electrode clamp (8) is provided at the other end of the copper rod (1); the tungsten electrode clamp (8) is connected to a tungsten electrode (11); an insulating gasket (9) is provided on the side of the tungsten electrode clamp (8) close to the copper rod (1); a circular gas nozzle (10) is provided on the side of the tungsten electrode clamp (8) close to the insulating gasket (9); the circular gas nozzle (10) does not contact the tungsten electrode clamp (8) and is fixedly connected to the lower cover (5) by an interference fit; The ultrasonic vibration system comprises an upper cover (2), wherein the upper cover (2) is fixedly connected to a transducer (3); the transducer (3) is fixedly connected to a split-type horn (4); the upper cover (2) is fixedly connected to an upper cover (7); and holes are opened at the axis of the ultrasonic vibration system for installing a TIG welding system.
2. The variable focus ultrasonic-TIG coaxial hybrid welding device according to claim 1 is characterized in that: The split-type horn (4) is a split-type concave spherical horn; it comprises a vibration receiving end (401) and an energy transmitting end (402), the vibration receiving end (401) and the energy transmitting end (402) being fixedly connected via threads; the energy transmitting end (402) is a concave spherical end surface; an insulating ring (403) and an annular water cooling groove (404) are provided at a node position of the split-type horn (4).
3. The variable focus ultrasonic-TIG coaxial hybrid welding device according to claim 1, characterized in that: The inner wall of the insulating ring (403) has symmetrical fan-shaped holes on both sides; the insulating ring (403) is made of ceramic material.
4. The variable focus ultrasonic-TIG coaxial hybrid welding device according to claim 1, characterized in that: The current circuits of the TIG welding system and the ultrasonic vibration system are independent of each other.
5. A welding method using the welding device according to any one of claims 1 to 4, characterized in that: The steps include: Step 1: Pre-welding treatment of workpiece; Step 2: Select the horn transmitting end according to the material of the workpiece to be welded and the form of the welding joint, and adjust the nozzle height; Step 3: Turn on water cooling and air cooling, perform ordinary TIG welding and then ultrasonic welding to obtain a high-performance welded joint.
6. The welding method according to claim 5, characterized in that: The step 1 specifically includes: before welding, the burrs, oxide layer and oil stains on the surface of the workpiece to be welded are fully cleaned, and the workpiece to be welded is fixed.
7. The welding method according to claim 5, characterized in that: The step 2 is specifically as follows: adjusting the position of the welding gun on the automatic walking device, selecting a variable amplitude rod transmitting end with a suitable diameter and curvature radius according to the material of the workpiece to be welded and the form of the welding joint, making the distance between the welding area of the workpiece to be welded and the concave end face of the variable amplitude rod be the focal length position of the sound field, and adjusting the nozzle height so that the tungsten electrode extends 4 to 6 mm outside the nozzle.
8. The welding method according to claim 5, characterized in that: The step 3 is specifically as follows: adjusting and determining the parameters of the welding power supply and the ultrasonic power supply, passing the welding shielding gas, opening the water cooling valve and the air cooling valve, performing ordinary TIG welding, and then turning on the ultrasonic power supply for ultrasonic-assisted welding to obtain a high-performance welded joint. After the welding is completed, first turning off the welding power supply, and then turning off the ultrasonic power supply.
Citation Information
Cited By
Electric arc additive manufacturing method for assisting in titanium alloy grain refinement through coaxial ultrasound
CN119634891A