Vacuum hot-pressing patching and repairing method for aircraft titanium alloy lower earring part
Through vacuum hot pressing and patching repair technology, the deformation and wear of the earring parts under titanium alloy during use is solved, the repair quality and mechanical properties are improved, the cost and scrap rate are reduced, and the stability and reliability of the aircraft are ensured.
Patent Information
- Application Number
- CN202411049583.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Aircraft titanium alloy earring parts are prone to deformation, wear and break during use. Conventional repair methods such as argon arc welding have the risk of missing welding, low weld strength, easy oxidation and large deformation, resulting in poor repair quality.
Using vacuum hot press patching repair method, through mechanical polishing and processing of conical bevels, vacuum hot press repair is performed using a blank of the same material as titanium alloy, multi-stage pressure and oscillation pressure are applied, and repaired in combination with vacuum and heating, and without loss Inspection ensures repair quality.
It improves the mechanical properties of the earrings under titanium alloy, reduces the repair cost, ensures the reliability of the aircraft, significantly reduces the scrap rate, and improves the repair quality.
Smart Images

Figure CN118989859A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of remanufacturing, and in particular to a vacuum hot-pressing patching and repairing method for a titanium alloy lower earring part of an aircraft. Background Art
[0002] The lower earring of the aircraft rudder is made of titanium alloy. This part is installed between the rudder and the vertical tail. One end of the lower earring with a bearing is connected to the rudder, and the two ears at the other end are fixed to the vertical tail through bolts. The earring mainly serves to connect and fix the rudder. Its structural diagram is shown in the figure below. Figure 1 As shown. The titanium alloy lower earrings may deform, wear, break, etc. during use, especially the inner side of the two circular lugs connected to the vertical tail, which will be significantly deformed due to wear and tension, affecting the stable flight of the aircraft. TIG welding is usually used to repair damage to this part, but due to the certain depth of the lug, there is a risk of leakage during surfacing welding. At the same time, the weld strength is low, it is very easy to oxidize, and the welding deformation is large. Summary of the invention
[0003] In view of the above situation, the present invention proposes a vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts, so as to solve the problems of low strength, easy oxidation, large deformation, high scrap rate, etc. of damaged aircraft lower earring products repaired by conventional means.
[0004] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0005] A vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts comprises the following steps:
[0006] S1. According to the damage, first mechanically grind and remove the deformed and worn parts around the titanium alloy lower earring lug, then process the titanium alloy lower earring lug from the outside to the inside into a tapered groove, clean the groove surface, soak the titanium alloy lower earring in acetone, and proceed to the next step within 12 hours;
[0007] S2. Use titanium alloy material that is the same as or similar to the titanium alloy lower earring to process a blank that matches the shape of the groove of the titanium alloy lower earring. The blank is a combination of a cylindrical and a conical structure. After cleaning and polishing the surface of the blank, soak it in acetone and proceed to the next step within 12 hours.
[0008] S3. Insert the cylindrical section of the blank from the large end face of the groove of the titanium alloy lower earring and press it, then put it into the vacuum hot pressing equipment, fix it with a clamp, and perform vacuum hot pressing repair. The vacuum hot pressing repair process is as follows:
[0009] First, evacuate the material, and when the vacuum degree reaches below 1Pa, start heating, heating to 800℃-1100℃ at a heating rate of 25℃ / min. While heating, simultaneously apply pressure to the upper and lower ends of the blank. The pressure is divided into three stages: first, 20MPa, hold the pressure for 2h, then increase the pressure to 40MPa, hold the pressure for 1h, and then increase the pressure to 50MPa, hold the pressure for 0.5h. During the holding process, an oscillating pressure with an amplitude of 2-6MPa and a frequency of 2-20Hz is applied;
[0010] S4. Cool down after vacuum hot pressing repair, release the pressure after cooling, take out the repaired titanium alloy lower earring for non-destructive testing. If there is no crack or pore inside, it is qualified. Re-drill the hole according to the drawing requirements and restore the part size. If there is crack or pore inside, it is unqualified. Repeat S1 to S3 until it is qualified.
[0011] Preferably, the angle of the tapered groove in S1 is less than 60°, and the size of the small end face of the tapered groove is determined according to the maximum radial size of the inner side of the titanium alloy lower earring after grinding.
[0012] Preferably, the titanium alloy material in S2 includes TA15 or TC4.
[0013] Preferably, the diameter of the large end face of the conical section of the blank in S2 is 1-2 mm larger than the diameter of the large end face of the groove of the titanium alloy lower earring connecting ear, the diameter of the small end face of the conical section of the blank is the same as the diameter of the small end face of the groove of the titanium alloy lower earring connecting ear, and the height dimension between the large and small end faces of the conical section of the blank is slightly larger than the thickness dimension of the titanium alloy lower earring connecting ear.
[0014] Preferably, the height dimension of the cylindrical section of the blank in S2 is 2-3 mm, and the diameter dimension of the cylindrical section of the blank is the same as the diameter dimension of the small end face of the conical section of the blank.
[0015] Preferably, in S4, the temperature is cooled at a rate of 3-10°C / s, and the pressure is released when the temperature drops to 500°C.
[0016] Preferably, the nondestructive testing method in S4 is fluorescent testing.
[0017] The beneficial effects of the present invention are:
[0018] The invention solves the problems of low strength, easy oxidation, large deformation, high scrap rate, etc. of damaged lower earring products repaired by conventional means, improves the mechanical properties of the lower earrings of aircraft, ensures the reliability of aircraft, reduces costs, and has extremely high economic and quality benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The present invention is further described below in conjunction with the accompanying drawings and embodiments:
[0020] Figure 1This is a schematic diagram of the structure of the titanium alloy lower earring parts of an aircraft;
[0021] Figure 2 is a flow chart of the present invention;
[0022] Figure 3 This is a schematic diagram of the ear groove structure of the titanium alloy lower earring part of the aircraft;
[0023] Figure 4 This is a schematic diagram of the structure for repairing bad materials. DETAILED DESCRIPTION
[0024] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0025] like Figure 2 As shown, a vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts comprises the following steps:
[0026] S1. According to the damage, the deformed and worn parts around the titanium alloy lower earring are first mechanically polished and removed, and then the titanium alloy lower earring is processed from the outside to the inside into a tapered groove. The groove structure is shown in Figure 3 The angle of the conical groove is less than 60°, and the small end face size of the conical groove is determined by the maximum radial size after the inner side of the titanium alloy lower earring is polished. After the groove surface is cleaned, the titanium alloy lower earring is immersed in acetone to avoid surface contamination, and the next step is performed within 12 hours.
[0027] S2. Use the same or similar titanium alloy material as the titanium alloy lower earring to process a blank that matches the shape of the titanium alloy lower earring bevel. The blank structure is shown in Figure 4 . Titanium alloy materials include TA15 or TC4. The blank is a combination of cylindrical and conical structures. The diameter of the large end face of the conical section of the blank is 1-2mm larger than the diameter of the large end face of the groove of the titanium alloy lower earring lug. The diameter of the small end face of the conical section of the blank is the same as the diameter of the small end face of the groove of the titanium alloy lower earring lug. The height dimension between the large and small end faces of the conical section of the blank is slightly larger than the thickness dimension of the titanium alloy lower earring lug. The height dimension of the cylindrical section of the blank is 2-3mm, and the diameter dimension of the cylindrical section of the blank is the same as the diameter dimension of the small end face of the conical section of the blank. After the blank is processed, it is pickled to remove surface oil, and then the blank is immersed in acetone and the next step is carried out within 12 hours.
[0028] S3. Insert the cylindrical section of the blank from the large end face of the groove of the titanium alloy lower earring and press it, then put it into the vacuum hot pressing equipment, fix it with a clamp, and perform vacuum hot pressing repair. The vacuum hot pressing repair process is as follows:
[0029] First, evacuate the material, and when the vacuum degree reaches below 1Pa, start heating, heating to 800℃-1100℃ at a heating rate of 25℃ / min. While heating, simultaneously apply pressure to the upper and lower ends of the billet. The pressure is divided into three sections. First, it is 20MPa, maintained for 2h, then increased to 40MPa, maintained for 1h, and then increased to 50MPa, maintained for 0.5h. During the pressure holding process, an oscillating pressure with an amplitude of 2-6MPa and a frequency of 2-20Hz is applied.
[0030] S4. After vacuum hot pressing repair, cool down at a rate of 3-10℃ / s. Release the pressure when the temperature drops to 500℃. Take out the repaired titanium alloy lower earring for non-destructive testing. The non-destructive testing method is fluorescent testing. If there is no crack or pore inside, it is qualified. Re-drill the hole according to the drawing requirements and restore the part size. If there is crack or pore inside, it is unqualified. Repeat S1 to S3 until it is qualified.
[0031] The present invention is further described in detail with reference to the following specific examples.
[0032] Embodiment 1
[0033] S1. Observe the damage of the circular ear of the titanium alloy lower earring part of the aircraft, especially the deviation of the hole at the ear from the specified value (thickness is 8mm, hole diameter is 10mm). Grind and remove the damaged part of the ear and open a tapered groove. The depth of the tapered groove is 8mm, the large end face diameter is 20mm, and the small end face diameter is 11mm. Then clean it and the groove structure is shown. Figure 3 .
[0034] S2. Use TA15 titanium alloy to process a blank that matches the groove of the lower earring and clean it. The structure of the blank is shown in Figure 4 The cylindrical section has a height of 2mm and a diameter of 11mm, and the conical section has a large end diameter of 21mm and a height of 9mm.
[0035] S3. Assemble the bad material with the lower earring bevel, then put it into the vacuum hot pressing equipment and fix it with a clamp. Close the hatch and start vacuuming. When the vacuum degree reaches below 1Pa, start heating, heating to 800℃ at a heating rate of 25℃ / min. While heating, apply pressure to the upper and lower ends of the bad material at the same time. The pressure is divided into three stages. First, maintain the pressure at 20MPa for 2h; then increase the pressure to 50MPa and maintain the pressure for 1h; then increase the pressure to 60MPa and maintain the pressure for 0.5h. During the pressure holding process, an oscillating pressure with an amplitude of 5MPa and a frequency of 2Hz is also applied.
[0036] S4. After cooling, take out the repaired lower earring for fluorescent flaw detection. If there are no defects such as cracks, machine it according to the requirements of the drawing, re-drill the hole, and restore the part size. If there are defects such as cracks, repeat S1 to S3 until it is qualified.
[0037] Embodiment 2
[0038] The difference from the first embodiment is that in S3 of this embodiment, the temperature is heated to 900° C. at a heating rate of 25° C. / min, and the amplitude of the oscillation pressure during the pressure holding process is 3 MPa.
[0039] Embodiment 3
[0040] The difference from the first and second embodiments is that the large end face diameter of the groove in S1 of this embodiment is 18 mm, and the large end face diameter of the tapered section of the material in step S2 is 20 mm and the height is 8 mm.
[0041] According to the above three embodiments, tensile specimens were prepared in the same way to verify the mechanical properties. The specific preparation method is: select a plate with the same thickness as the part, with a length and width of 200 mm and 50 mm respectively, open a tapered hole in the center of the plate as in the embodiment, process the same blank, then perform vacuum hot pressing patching, and process the patched plate into a tensile specimen. The plate size is designed according to GB / T228.1.
[0042] At the same time, a comparison of manual tungsten inert gas arc welding repair was also carried out. The specific process is: select a plate with the same thickness as the part, with a length and width of 200mm and 50mm respectively, open a hole in the center of the plate, the diameter of the hole is the same as the circular hole of the part, and open a groove around the hole for a smooth transition. After the area around the hole is polished clean, the hole is blocked by argon arc welding. When blocking the hole, a titanium alloy plate is first placed under the small end face, and then surfacing welding is started. The welding current is 80A and the welding wire is TA15. After welding, the plate is processed into a tensile specimen for mechanical property testing. The test results are shown in Table 1.
[0043] Table 1 Performance test table of different repair methods
[0044]
[0045] As can be seen from Table 1, the mechanical properties of the products repaired by vacuum hot pressing are similar to those of the parent material and significantly higher than those of the samples repaired by argon arc welding.
[0046] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts, characterized in that: The following steps are involved: S1. According to the damage, first mechanically grind and remove the deformed and worn parts around the titanium alloy lower earring lug, then process the titanium alloy lower earring lug from the outside to the inside into a tapered groove, clean the groove surface, soak the titanium alloy lower earring in acetone, and proceed to the next step within 12 hours; S2. Use titanium alloy material that is the same as or similar to the titanium alloy lower earring to process a blank that matches the shape of the groove of the titanium alloy lower earring. The blank is a combination of a cylindrical and a conical structure. After cleaning and polishing the surface of the blank, soak it in acetone and proceed to the next step within 12 hours. S3. Insert the cylindrical section of the blank from the large end face of the groove of the titanium alloy lower earring and press it, then put it into the vacuum hot pressing equipment, fix it with a clamp, and perform vacuum hot pressing repair. The vacuum hot pressing repair process is as follows: First, evacuate the vacuum, and when the vacuum degree reaches below 1Pa, start heating, heating to 800℃-1100℃ at a heating rate of 25℃ / min. While heating, simultaneously apply pressure to the upper and lower ends of the billet. The pressure is divided into three stages, first 20MPa, hold the pressure for 2h, then increase the pressure to 40MPa, hold the pressure for 1h, then increase the pressure to 50MPa, hold the pressure for 0.5h, and apply an oscillating pressure with an amplitude of 2-6MPa and a frequency of 2-20Hz while holding the pressure; S4. Cool down after vacuum hot pressing repair, release the pressure after cooling, take out the repaired titanium alloy lower earring for non-destructive testing. If there is no crack or pore inside, it is qualified. Re-drill the hole according to the drawing requirements and restore the part size. If there is crack or pore inside, it is unqualified. Repeat S1 to S3 until it is qualified.
2. The vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts according to claim 1 is characterized in that: The angle of the tapered groove in S1 is less than 60°, and the small end face size of the tapered groove is determined by the maximum radial size after the inner side of the titanium alloy lower earring is polished.
3. The vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts according to claim 1 is characterized in that: The titanium alloy materials in S2 include TA15 or TC4.
4. The vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts according to claim 1 is characterized in that: The large end face diameter of the conical section of the blank in S2 is 1-2 mm larger than the large end face diameter of the titanium alloy lower earring connecting groove, the small end face diameter of the conical section of the blank is the same as the small end face diameter of the titanium alloy lower earring connecting groove, and the height dimension between the large and small end faces of the conical section of the blank is slightly larger than the thickness dimension of the titanium alloy lower earring connecting groove.
5. The vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts according to claim 1 is characterized in that: The height dimension of the cylindrical section of the blank in S2 is 2-3 mm, and the diameter dimension of the cylindrical section of the blank is the same as the diameter dimension of the small end face of the conical section of the blank.
6. The vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts according to claim 1 is characterized in that: In S4, the temperature is cooled at a rate of 3-10°C / s, and the pressure is released when the temperature drops to 500°C.
7. The vacuum hot pressing patching and repairing method for aircraft titanium alloy lower earring parts according to claim 1 is characterized in that: The non-destructive testing method in S4 is fluorescent testing.
Citation Information
Patent Citations
Compound repair method and repair material for high-temperature alloy
CN109848638A
Composite repairing method for damage of high-temperature alloy casing
CN113843576A
On-line repair welding process for cracking of metal flange hole bridge
CN114939770A
Repair method for high-temperature component and repaired high-temperature component
JP2003176727A
Method for remanufacturing flywheel
US20160195163A1