Preparation method of Ti-6Al-4V titanium alloy small and medium-sized bars with reduced cost
Through the combined process of large deformation, length extraction and forging and low-temperature rolling, the problem of processing difficulty and high cost of small-sized rods of Ti-6Al-4V titanium alloy is solved, and the preparation of tissue uniformity and stable performance is achieved, reducing production costs and cycle, suitable for industrial production.
Patent Information
- Application Number
- CN202410953277.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
Ti-6Al-4V titanium alloy is difficult to process and has high cost, resulting in poor market competitiveness. Especially when preparing small-sized bars, it is difficult to control the composition uniformity, and the processing window is narrow. Traditional technology requires multiple fires to be free forged and repaired. Grinding leads to large material loss and long cycle.
The original cast structure is crushed by large deformation, continuous lengthening forging, and the microstructure is improved by low temperature continuous lengthening forging, and rolling is carried out below the β phase transformation point. Combined with the parallel and axial lengthening process, the rolling temperature and ratio are controlled to reduce Fire and grinding times.
It realizes the uniform structure and stable performance of Ti-6Al-4V titanium alloy small-sized rods, reduces production costs, shortens cycles, improves yield and production efficiency, and is suitable for industrial production.
Smart Images

Figure CN118989865A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonferrous metal material processing, and relates to a method for preparing Ti-6Al-4V titanium alloy small and medium-sized bars with reduced cost. Background Art
[0002] Ti-6Al-4V titanium alloy, which belongs to α+β titanium alloy, has good comprehensive mechanical properties and is widely used all over the world. It can be used as engine drums, disks, blades, etc. It can also be used to make flanges, housings, sealing gaskets, etc. However, due to the poor plasticity and high temperature sensitivity of titanium alloy, the processing window is narrow and the processing is difficult. After the ingot is opened, it needs multiple free forging and grinding. The processing cost is high, the cycle is long, and the material loss is large, resulting in high comprehensive cost and poor market core competitiveness.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to overcome the disadvantages of the prior art and provide a method for preparing small and medium-sized (Φ≤120mm) Ti-6Al-4V titanium alloy bars with reduced cost.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] This method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced costs includes: first, large deformation drawing forging is used to open the ingot to fully break the original cast structure, and air cooling is performed after the drawing forging is completed to obtain a fine β-structured billet; then, a drawing spring anvil is used for low-temperature continuous drawing forging below the β phase transformation point to make the billet into a short rod shape and improve the bar microstructure; finally, at least one fire rolling is performed below the β phase transformation point temperature to complete the preparation of small and medium-sized titanium alloy bars.
[0007] Specifically, the preparation method comprises the following steps:
[0008] Step 1, blank forging: sawing and dividing the ingot according to the weight of the ingot, the weight of a single billet is 2500kg-3700kg, and the single ingot blank forging adopts only large deformation drawing forging, and the drawing process adopts the horizontal drawing parallel to the anvil and the axial drawing perpendicular to the anvil combined forging, and the drawing ratio is 5.8-9.0, so as to fully break the original cast structure of the billet and obtain a billet with uniform and fine β structure of 2mm-3.5mm;
[0009] Step 2, low temperature drawing of the intermediate billet: using a drawing spring anvil to perform low temperature continuous drawing forging on the billet at a temperature below the β phase transformation point;
[0010] Step 3: Low temperature rolling forming: Use a corresponding rolling mill to perform at least one hot rolling at a temperature below the β phase transformation point until the target size is reached, thereby completing the preparation of small and medium-sized titanium alloy bars.
[0011] Specifically, in step 1, the single ingot blank forging adopts one fire large deformation stretching, the heating temperature is 1150° C. to 1180° C., and the heating coefficient is 0.65 min / mm to 0.80 min / mm.
[0012] Specifically, a resistance furnace or a natural gas furnace is used for heating.
[0013] Specifically, in step 2, a drawing spring anvil is used to perform low temperature continuous drawing forging on the blank at a temperature below the β phase transformation point, specifically:
[0014] The blank is subjected to low temperature drawing forging at 40°C to 50°C below the β phase transformation point, and the heating coefficient is 0.60min / mm to 0.75min / mm;
[0015] After forging is completed, the billet is reheated, the heating temperature is still 30°C to 50°C below the β phase transformation point temperature, the holding time is 60min to 180min, and the drawing is continued using a drawing spring anvil; wherein the drawing cumulative forging ratio is 3.8 to 4.8, and the billet is air-cooled after forging is completed.
[0016] Specifically, in step 3, the rolling is performed at 50°C to 70°C below the β phase transformation point, the insulation coefficient is 0.70min / mm to 0.80min / mm, the rolling ratio is ≥2.1, and the rolling is performed to the target size and then air-cooled.
[0017] Specifically, in step 3, after rolling is completed, residual temperature online straightening is used to control the curvature of the bar to ≤1 mm / m.
[0018] Specifically, the rolling ratio is 7.5 to 10.2.
[0019] Specifically, the ingot is an ingot with a diameter of 920 mm to 1050 mm obtained by multiple VAR smelting or EB+VAR smelting.
[0020] Specifically, the diameter of the titanium alloy small and medium-sized bars is Φ≤120 mm.
[0021] Compared with the prior art, the technical solution provided by the present invention includes the following beneficial effects: based on ingots with specifications of Ф920mm~Ф1050mm, the preparation method of Ti-6Al-4V titanium alloy small and medium-sized bars (Ф≤120mm) provided by the present invention overcomes the problem of difficulty in controlling composition uniformity caused by large-sized ingots in the existing preparation process, and can produce small and medium-sized bars (Ф≤120mm) that meet the requirements of technical standards, and have uniform structure and stable performance, reduce the number of fires and grinding / polishing in the existing preparation process, have low cost, and are suitable for industrial production.
[0022] Specifically: the present invention abandons the traditional process scheme of free forging and multi-fire upsetting of bars, and adopts large deformation stretching forging of ingot blanking. The stretching process adopts a combination of transverse stretching parallel to the anvil and axial stretching perpendicular to the anvil to fully break the original cast structure and obtain a fine β-structured billet; below the phase transformation point, stretching spring anvil forging is used to make the near-surface structure of the billet more refined and make it short rod-shaped, thereby improving the microstructure of the bar; through rolling forming, the core structure of the billet is improved, and the rolling process temperature and rolling ratio are controlled, so as to effectively achieve the refinement and uniformity of the bar structure and the consistency of the production process, and greatly improve the production efficiency and yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0025] Figure 1 A flow chart of a method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost provided by the present invention;
[0026] FIG2(a) is a low-magnification microstructure diagram of a Φ76.2 mm rod prepared in Example 1 of the present invention, and FIG2(b) and FIG2(c) are high-magnification microstructure diagrams of the same position (R / 2 in the transverse direction) of different Φ76.2 mm rods prepared in Example 1 of the present invention;
[0027] FIG3(a) is a low-magnification microstructure diagram of a Φ40 mm rod prepared in Example 1 of the present invention, and FIG3(b) and FIG3(c) are high-magnification microstructure diagrams of the same position (R / 2 in the transverse direction) of different Φ40 mm rods prepared in Example 1 of the present invention;
[0028] FIG4(a) is a low-magnification microstructure of a Φ120 mm rod prepared in Example 2 of the present invention, and FIG4(b) is a high-magnification microstructure of a Φ120 mm rod prepared in Example 2 of the present invention;
[0029] FIG5(a) is a macroscopic microstructure diagram of a Φ105 mm rod prepared in Example 2 of the present invention, and FIG5(b) is a macroscopic microstructure diagram of a Φ90 mm rod prepared in Example 2 of the present invention;
[0030] FIG6(a), FIG6(b), and FIG6(c) are respectively high-magnification microstructure images of the Φ26 mm rod prepared in Example 3 of the present invention at different magnifications. DETAILED DESCRIPTION
[0031] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention described in detail in the appended claims.
[0032] The present invention provides a method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced costs, using multiple VAR smelting or EB+VAR smelting of Ф920mm~Ф1050mm ingots to produce bars with Ф≤120mm that meet technical standards, with uniform structure, excellent performance, low cost, and suitable for industrial production. The specific steps of the preparation method are as follows, see Figure 1 As shown:
[0033] Step 1, open forging: the ingot is heated by a resistance furnace or a natural gas furnace, the opening heating temperature is 1150℃~1180℃, and the heating coefficient is 0.65min / mm~0.80min / mm; the ingot open forging only adopts drawing forging, the weight of a single billet after material separation is 2500kg~3700kg, the whole billet is only drawn, and the drawing forging ratio is 5.8~9.0; in order to improve the drawing efficiency, the drawing process adopts the horizontal drawing parallel to the anvil and the axial drawing perpendicular to the anvil combined with forging, shortening the forging time, so as to increase the final forging temperature, and air cooling after forging. After the open forging, the original cast structure of the billet is fully broken, and a billet with uniform and fine β structure of 2mm~3.5mm is obtained.
[0034] Specifically, the heating and holding time can be calculated by the heating coefficient, and the empirical formula is: T = αD, where α is the heating coefficient and D is the effective thickness of the forging blank.
[0035] Step 2, low-temperature drawing of the intermediate billet: heating and drawing forging at 40°C to 50°C below the β phase transformation point, the heating coefficient is 0.60min / mm to 0.75min / mm, and the drawing spring anvil is used for forging. The drawing forging ratio is 2.0 to 2.3. After forging, the billet is reheated, the heating temperature remains unchanged, and the holding time is 60min to 180min. After reaching the temperature, the drawing is continued, the drawing forging ratio is 1.9 to 2.1, and the cumulative forging ratio is 3.8 to 4.8, so as to improve the drawing efficiency and uniformity of the bar. After forging, the billet is air-cooled.
[0036] Step 3, low temperature rolling forming: heating rolling at 50℃~70℃ below the β phase transformation point, with a heat preservation coefficient of 0.70min / mm~0.80min / mm, a rolling ratio ≥2.1, rolling to the target size through 1 or 2 passes, straightening the bar online with residual temperature after rolling, controlling the curvature of the bar to be ≤1mm / m, and air cooling after straightening.
[0037] The finished bar size is determined by the final saleable or usable finished product size, taking into account the oxide scale thickness and adding the processing allowance. The bars formed by rolling are then processed by a subsequent heat treatment machine to remove the oxide scale on the outer surface and both ends of the bars to become the final product.
[0038] Through the above-mentioned method, the preparation method of small and medium-sized Ti-6Al-4V titanium alloy bars provided by the present invention abandons the traditional free forging multi-fire upsetting and drawing process scheme, and adopts the large deformation drawing forging of the ingot to fully break the original cast structure to obtain a fine β-structured billet; below the phase transformation point, the drawing spring anvil forging is used to make the near-surface structure of the billet more refined and short-bar-shaped, thereby improving the microstructure of the bar; through rolling forming, the core structure of the billet is improved, the rolling process temperature and rolling ratio are controlled, and the uniformity of the bar structure and the consistency of the production process are effectively achieved, and the production efficiency and yield rate are greatly improved. By controlling the curvature of the bar, the machining allowance is reduced and the material utilization rate is improved. By adopting the preparation method of the present invention, the yield rate is increased by about 4.2%, the heating forging fire is reduced, the hot processing cost is reduced by 38%, and the production cycle is shortened by 40%.
[0039] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0040] Example 1
[0041] This embodiment provides a method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost, comprising the following steps:
[0042] Step 1, blank forging: the ingot specification is 920mm, the β phase transformation point of the ingot is 990℃, the weight of a single billet after the ingot is divided into three equal parts is 2500kg, and a natural gas furnace is used for heating. The blank heating temperature is 1150℃, the heating coefficient is 0.65min / mm, and only the drawing forging process is used, and the drawing forging ratio is 5.8; the drawing process first adopts the transverse drawing parallel to the anvil, and the transverse drawing can increase the deformation of the core of the billet, and the drawing efficiency is high. When the billet length exceeds the transverse length of the flat anvil, the axial drawing forging is combined, thereby shortening the forging time and increasing the final forging temperature. The billet is air-cooled after forging to ensure that the original cast structure is fully broken to obtain a billet with uniform and fine β structure of 2mm to 3.5mm.
[0043] Step 2, low-temperature drawing of the intermediate billet: heating and drawing at 40°C below the β phase transformation point temperature, that is, the temperature is set to 950°C, the heating and insulation coefficient is 0.75min / mm, and the drawing spring anvil is used for forging. The drawing and forging ratio is 2.3. After forging, the billet is reheated, the heating temperature is 960°C, the insulation time is 60min, and the drawing is continued. The drawing and forging ratio is 1.9, the cumulative forging ratio is 4.4, and the billet is air-cooled after forging.
[0044] Step 3, low temperature rolling forming: heating at 60°C below the β phase transformation point, the heating temperature is 930°C, the insulation coefficient is 0.75min / mm, the billet is rolled into finished bars of different specifications, the Φ81mm bar is rolled into one fire, the rolling ratio is 4.9, the Φ44mm bar is rolled into two fires, after the forming is completed, the residual temperature is used for online straightening, and the curvature of the bar is ≤1mm / m.
[0045] The rods are machined by machining equipment to remove the oxide scale on the outer surface and both ends, and the dimensions are processed at the same time. The dimension processing includes the outer diameter and length to obtain the final titanium alloy rods of Φ76.2mm and Φ40mm.
[0046] The room temperature mechanical properties of the Φ76.2mm titanium alloy rods prepared in Example 1 with different section numbers after heat treatment are shown in Table 1 below. The results show that the rods all meet the requirements and have a certain margin and a small range, and have good stability in mass production. Figure 2(a) is a low-magnification microstructure diagram of a typical Φ76.2mm rod, Figure 2(b) and Figure 2(c) are high-magnification microstructure diagrams of the same position (R / 2 - transverse) of different Φ76.2mm rods prepared in this example, Figure 3(a) is a low-magnification microstructure diagram of the Φ40mm rod prepared in this example, Figure 3(b) and Figure 3(c) are high-magnification microstructure diagrams of the same position (R / 2 - transverse) of different Φ40mm rods prepared in this example. Figure 2(a) to Figure 2(c) ,Depend on Figure 3(a) to Figure 3(c)It can be seen that the titanium alloy rod prepared in Example 1 has no continuous grain boundaries in its microstructure and has good uniformity.
[0047] Table 1 Mechanical properties of rods
[0048]
[0049] Example 2
[0050] This embodiment provides another method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost, comprising the following steps:
[0051] Step 1, blank forging: the ingot specification is Ф1020mm, the ingot β phase transformation point is 995℃, the weight of a single blank after the ingot is divided into three equal parts is 3200kg, and the resistance furnace is used for heating. The blank heating temperature is 1170℃, the heating coefficient is 0.75min / mm, and only the drawing forging process is used, and the drawing forging ratio is 8.5; the drawing process first adopts the transverse drawing parallel to the anvil, and when the billet length exceeds the transverse length of the flat anvil, the axial drawing forging is combined, thereby shortening the forging time and increasing the final forging temperature. The billet is air-cooled after forging to ensure that the original cast structure is fully broken to obtain a billet with uniform and fine β structure of 2mm to 3.5mm.
[0052] Step 2, low-temperature drawing of the intermediate billet: heating and drawing at 50°C below the β phase transformation point temperature, that is, the temperature is set to 945°C, the heating and insulation coefficient is 0.65min / mm, and the drawing spring anvil is used for forging. The drawing and forging ratio is 2.0. After forging, the billet is reheated, the heating temperature is 945°C, the insulation time is 120min, and the drawing is continued. The drawing and forging ratio is 2.0, the cumulative forging ratio is 4.0, and the billet is air-cooled after forging.
[0053] Step 3, low temperature rolling forming: heating at 55 ° C below the β phase transformation point temperature, the heating temperature is 940 ° C, the insulation coefficient is 0.80 min / mm, the billet is rolled into finished bars of different specifications, and the bars of Φ125mm, Φ110mm, and Φ95mm specifications are all rolled in one fire, and the rolling ratios are 2.1, 2.9, and 3.6 respectively. After forming, the residual temperature is used for online straightening, and the curvature of the bar is ≤1mm / m.
[0054] The rods are machined by machining equipment to remove the oxide scale on the outer surface and both ends, and the dimensions are processed at the same time. The dimension processing includes the outer diameter and length to obtain the final titanium alloy rods of Φ120mm, Φ105mm and Φ90mm.
[0055] The room temperature mechanical properties of the Φ120mm titanium alloy rod obtained in Example 2 in different directions after heat treatment are shown in Table 2 below. The extreme difference in the horizontal and vertical directions is small, indicating that the organization is uniform and there is no anisotropy. Table 3 shows the room temperature mechanical properties of the Φ90mm titanium alloy rod obtained in Example 2 at different positions and directions of the rod after heat treatment. The results all meet the requirements and have a certain margin, and the extreme difference in the horizontal and vertical directions at different positions is small, the organization is uniform, and there is no anisotropy. Figure 4 (a) is the low-power organization of the Φ120mm rod prepared in Example 2, and Figure 4 (b) is the high-power microstructure of the Φ120mm rod prepared in this example. It can be seen from Figures 4 (a) and 4 (b) that there is no continuous grain boundary in its microstructure. Figure 5 (a) is the low-power organization of the Φ105mm rod prepared in this example, and Figure 5 (b) is the low-power organization of the Φ90mm rod prepared in this example, all of which are fuzzy crystals. Generally speaking, fuzzy crystals have good toughness under high temperature and high stress, which can extend the service life of the material.
[0056] Table 2 Mechanical properties of Φ120mm bars
[0057]
[0058] Table 3 Mechanical properties of Φ90mm bars
[0059]
[0060] Example 3
[0061] This embodiment provides another method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost, comprising the following steps:
[0062] Step 1, blank forging: the ingot specification is Ф1050mm, the ingot β phase transformation point is 990℃, the weight of a single blank after the ingot is divided into three equal parts is 3700kg, and a natural gas furnace is used for heating. The blank heating temperature is 1180℃, the heating coefficient is 0.80min / mm, and only the drawing forging process is used, and the drawing forging ratio is 9.0; the drawing process first adopts the transverse drawing parallel to the anvil, and when the billet length exceeds the transverse length of the flat anvil, the axial drawing forging is combined, thereby shortening the forging time and increasing the final forging temperature. The billet is air-cooled after forging to ensure that the original cast structure is fully broken, and a billet with uniform and fine β structure of 2mm to 3.5mm is obtained;
[0063] Step 2, low-temperature drawing of the intermediate billet: heating and drawing at 45°C below the β phase transformation point temperature, that is, the temperature is set to 945°C, the heating and insulation coefficient is 0.60min / mm, and the drawing spring anvil is used for forging. The drawing and forging ratio is 2.0. After forging, the billet is reheated, the heating temperature is 950°C, the insulation time is 180min, and the drawing is continued. The drawing and forging ratio is 2.1, the cumulative forging ratio is 4.2, and the billet is air-cooled after forging.
[0064] Step 3, low temperature rolling forming: heating at 70℃ below the β phase transformation point, the heating temperature is 920℃, the insulation coefficient is 0.70min / mm, the billet is rolled into finished bars of different specifications, Φ43mm and Φ28mm bars are divided into 2 fires for rolling forming, the rolling ratio is ≥10, after forming, the residual temperature is used for online straightening, and the curvature of the bar is ≤1mm / m.
[0065] The rods are machined by machining equipment to remove the oxide scale on the outer surface and both ends, and the dimensions are processed at the same time. The dimension processing includes the outer diameter and length to obtain the final titanium alloy rods of Φ40mm and Φ26mm.
[0066] The longitudinal room temperature mechanical properties of different batches of Φ40mm and Φ26mm titanium alloy bars obtained in Example 3 after heat treatment are shown in Table 4 below. The results all meet the requirements and have a certain margin, and the range is small, and the batch production stability is good. Figure 6 (a), Figure 6 (b), and Figure 6 (c) are high-magnification microstructure diagrams of the Φ26mm bars prepared in this example at different magnifications, and it can be seen that there is no continuous grain boundary in the microstructure, and the uniformity is good.
[0067] Table 4 Mechanical properties of rods
[0068]
[0069] In summary, the present invention adopts an ingot with a specification of 920 mm to 1050 mm, and provides a method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars, and produces bars with a specification of 120 mm or less that meet the requirements of technical standards, with uniform structure, excellent performance, low cost, and suitable for industrial production. It should be noted that in actual production, the specifications of the ingots are not limited to 920 mm, 1020 mm, and 1050 mm, and the product grades are not limited to Ti-6Al-4V titanium alloys, and can be extended to other Ti-6Al-4VELI, TC4 alloys, etc. The finished bar size is not limited to the size specifications of the above-mentioned embodiment. Moreover, in actual production, the finished bar size can be calculated based on the final finished product delivery size, taking into account the oxide scale thickness and processing allowance generated during the forging process, and then the intermediate billet size can be calculated.
[0070] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0071] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost, It is characterized in that Firstly, the ingot is forged by large deformation drawing forging to fully break up the original cast structure. After the drawing forging is completed, it is air-cooled to obtain a billet with fine β structure. Then, a drawing spring anvil is used for low-temperature continuous drawing forging below the β phase transformation point to make the billet into a short rod shape and improve the microstructure of the rod. Finally, at least one fire rolling is carried out below the β phase transformation point to complete the preparation of small and medium-sized titanium alloy bars.
2. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 1, It is characterized in that The following steps are involved: Step 1, blank forging: sawing and dividing the ingot according to the weight of the ingot, the weight of a single billet is 2500kg-3700kg, and the single ingot blank forging adopts only large deformation drawing forging, and the drawing process adopts the horizontal drawing parallel to the anvil and the axial drawing perpendicular to the anvil combined forging, and the drawing ratio is 5.8-9.0, so as to fully break the original cast structure of the billet and obtain a billet with uniform and fine β structure of 2mm-3.5mm; Step 2, low temperature drawing of the intermediate billet: using a drawing spring anvil to perform low temperature continuous drawing forging on the billet at a temperature below the β phase transformation point; Step 3, low temperature rolling forming: use the corresponding rolling mill to carry out at least one hot rolling at a temperature below the β phase transformation point until the target size is reached, so as to complete the preparation of small and medium-sized titanium alloy bars.
3. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 2, It is characterized in that In step 1, the single ingot forging adopts one fire large deformation drawing, the heating temperature is 1150℃~1180℃, and the heating coefficient is 0.65min / mm~0.80min / mm.
4. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 3, It is characterized in that Heating is carried out using a resistance furnace or a natural gas furnace.
5. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 2, It is characterized in that In step 2, a drawing spring anvil is used to perform low temperature continuous drawing forging on the blank at a temperature below the β phase transformation point, specifically: The blank is subjected to low temperature drawing forging at 40°C to 50°C below the β phase transformation point, and the heating coefficient is 0.60min / mm to 0.75min / mm; After forging is completed, the billet is reheated, the heating temperature is still 30°C to 50°C below the β phase transformation point temperature, the holding time is 60min to 180min, and the drawing is continued using a drawing spring anvil; wherein the drawing cumulative forging ratio is 3.8 to 4.8, and the billet is air-cooled after forging is completed.
6. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 2, It is characterized in that In step 3, the rolling is performed at 50°C to 70°C below the β phase transformation point, the insulation coefficient is 0.70min / mm to 0.80min / mm, the rolling ratio is ≥2.1, and the rolling is performed to the target size and then air-cooled.
7. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 6, It is characterized in that In step 3, after rolling is completed, residual temperature online straightening is used to control the curvature of the bar to ≤1mm / m.
8. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to claim 6, It is characterized in that The rolling ratio is 7.5 to 10.
2.
9. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to any one of claims 1 to 8, It is characterized in that The ingot is an ingot with a diameter of 920 mm to 1050 mm obtained by VAR smelting or EB+VAR smelting.
10. The method for preparing small and medium-sized Ti-6Al-4V titanium alloy bars with reduced cost according to any one of claims 1 to 8, It is characterized in that The diameter of the titanium alloy small and medium-sized bars is Φ≤120mm.