Graphene-based heating and thermal insulation fabric
Through the core-shell double-layer electrospinning technology of modified graphene gel liquid and polyamide spinning liquid, combined with far-infrared fiber braiding, the problem of improving the warmth performance of the fabric is solved, and the efficient heating, moisture absorption and bacterial prevention of the fabric is achieved. The performance improvement significantly improves the overall performance of the fabric.
Patent Information
- Application Number
- CN202411073794.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is room for improvement in existing fabrics in terms of warmth performance, especially in combining graphene's high thermal conductivity and special biological properties, which have not fully realized their potential, and traditional composite materials have limited applications in the field of clothing.
The modified graphene gel liquid and polyamide spinning liquid were used to perform core-shell double-layer electrospinning to prepare graphene heat-absorbing composite yarn with core-shell composite structure, and woven with far-infrared fibers to form excellent heating and moisture absorbing properties of fabrics.
It achieves the high-efficiency far infrared heating and moisture absorption performance of the fabric, enhances the warmth effect of the fabric, and improves the antibacterial properties and the tensile strength of the fiber wire, significantly improving the overall performance of the fabric.
Smart Images

Figure BDA0004981627250000051 
Figure BDA0004981627250000061 
Figure BDA0004981627250000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabrics, and in particular relates to a graphene-based heat-generating and heat-insulating fabric. Background Art
[0002] For the fabrics used to make winter clothing, the most basic requirement is that they have good heat-retention and heat-insulating properties. There are many ways to improve the thermal insulation performance of fabrics, for example, improving the thermal insulation of fabrics by improving the weaving process of fabrics, developing thermal insulation fibers and using them to make fabrics, which have better thermal insulation than ordinary fibers, and thus enhancing the thermal insulation of fabrics. The thermal insulation of fabrics can also be improved by developing films with thermal insulation properties and compounding them with fabrics.
[0003] The existing technology for the development of thermal insulation fibers is mostly to mix materials with excellent heating properties into polymers and then obtain them through spinning. Graphene has high strength, high thermal conductivity, optical and electrical response properties, and special biological properties. In the field of clothing fabrics, compounding graphene with other polymer materials can give the composite materials new functions derived from the graphene itself, which can realize the upgrading and empowerment of traditional fabric products. To this end, we propose a heat-generating and thermal insulation fabric based on graphene. Summary of the invention
[0004] The purpose of the present invention is to provide a graphene-based heat-generating and thermal-insulating fabric in order to solve the above-mentioned problems.
[0005] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0006] The present invention provides a graphene-based heat-generating and heat-insulating fabric, which is woven from a surface fabric and a base fabric, wherein the surface fabric is woven using far-infrared fibers as warp and weft threads, and the base fabric is woven using graphene heat-generating and moisture-absorbing composite yarns as warp and weft threads;
[0007] The graphene exothermic and hygroscopic composite yarn is a core-shell composite fiber yarn obtained by core-shell double-layer electrospinning of modified graphene gel solution and polyamide spinning solution, and the mass ratio of the modified graphene gel solution to the polyamide spinning solution is 2:4-6.
[0008] As a further optimization scheme of the present invention, the preparation method of the modified graphene gel solution comprises the following steps:
[0009] (1) dispersing graphene in an acid solution, and separating and obtaining modified graphene after a rotational friction treatment for 30-60 min;
[0010] (2) adding the modified graphene and boric acid into the polypyrrole gel and uniformly dispersing them by ultrasonication, then adding distilled water and continuously ultrasonicating until a slurry is formed, and then distilling under reduced pressure to obtain a modified graphene gel solution.
[0011] As a further optimization scheme of the present invention, the mass ratio of the modified graphene, boric acid and polypyrrole gel is 3:0.5:1, and the amount of distilled water added is 300% of the mass of the modified graphene.
[0012] As a further optimization scheme of the present invention, the polyamide spinning solution comprises, by mass percentage, 35-45% polyamide, 6-10% hydroxy silicone oil, 2-4% kaolin, and the remainder is solvent.
[0013] As a further optimization scheme of the present invention, the electrospinning adopts a coaxial electrospinning device, and the coaxial electrospinning device has a coaxial needle with a double-layer structure of a shell layer needle cavity and a core layer needle cavity. The shell layer needle cavity is connected to the shell layer syringe through an injection tube, and the core layer needle cavity is connected to the core layer syringe through an injection tube. The modified graphene gel liquid is used as the core layer spinning liquid, and the polyamide spinning liquid is used as the shell layer spinning liquid.
[0014] As a further optimization scheme of the present invention, the parameters of the electrospinning are: working voltage of 15-20 kV, receiving distance of 12-15 cm, temperature of 100-110° C., core solution propulsion rate of 0.1-2 ml / h, and shell solution propulsion rate of 0.1-3 ml / h.
[0015] As a further optimization scheme of the present invention, the far-infrared fiber is prepared by uniformly mixing dry polyurethane slices with far-infrared ceramic powder, antistatic agent and dispersant, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch and melt-spinning to obtain the far-infrared fiber.
[0016] The beneficial effects of the present invention are:
[0017] 1. The present invention uses far-infrared fibers as warp and weft to weave a surface fabric, and then uses graphene heating and hygroscopic composite yarns as warp and weft to weave a base fabric, and then weaves the surface fabric and the base fabric to obtain a fabric, which has excellent thermal insulation and heating properties. The far-infrared fibers enable the fabric to have good far-infrared heating properties, and the graphene heating and hygroscopic composite yarns with a core layer double-layer structure enable the fabric to have both heating properties and hygroscopic properties.
[0018] 2. The present invention obtains modified graphene by treating graphene with an acid solution combined with a rotary friction treatment, thereby improving the hydrophilicity and lamellae state of the graphene, enhancing the dispersibility of the graphene, and promoting the full play of its own heating performance, so that the fabric has better hygroscopic heat generation and antibacterial properties. DETAILED DESCRIPTION
[0019] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0020] Example 1
[0021] This embodiment provides a graphene-based heat-generating and heat-insulating fabric, which is woven from a surface fabric and a base fabric, wherein the surface fabric is woven using far-infrared fibers as warp and weft threads, and the base fabric is woven using graphene heat-generating and moisture-absorbing composite yarns as warp and weft threads;
[0022] The graphene exothermic and hygroscopic composite yarn is a core-shell composite fiber yarn obtained by core-shell double-layer electrostatic spinning and curing of modified graphene gel solution and polyamide spinning solution, and the mass ratio of the modified graphene gel solution to the polyamide spinning solution is 2:4.
[0023] In this embodiment, the far-infrared fiber is prepared by uniformly mixing 90% of dry polyurethane chips with 8% of far-infrared ceramic powder, 1% of antistatic agent (ethoxylated lauryl amide) and 1% of dispersant NNO, and granulating the mixture to obtain a far-infrared masterbatch. The far-infrared masterbatch is dried and melt-spun to obtain the far-infrared fiber (melt spinning is a well-known technique for those skilled in the art, and this embodiment does not improve it, so it is not limited thereto).
[0024] Among them, the preparation method of modified graphene gel solution is as follows: graphene is dispersed in a p-hydroxycinnamic acid solution (in this embodiment, the mass volume ratio of graphene to p-hydroxycinnamic acid is 1g:10ml), and modified graphene is separated after rotational friction treatment for 30 minutes under a load of 100N and a rotation speed of 10r / s, and then the modified graphene and boric acid are added to the polypyrrole gel for ultrasonic dispersion, and then distilled water is added and continuously ultrasonicated to form a slurry, and the modified graphene gel solution is obtained after reduced pressure distillation. The mass ratio of the modified graphene, boric acid and polypyrrole gel is 3:0.5:1, the amount of distilled water added is 300% of the mass of the modified graphene, the frequency of the ultrasound is 40kHz, the temperature is 40°C, the temperature of the reduced pressure distillation is 120°C, the pressure is 80% of the atmospheric pressure, and the volume of the modified graphene gel solution is 30% of the solution before reduced pressure distillation.
[0025] The polyamide spinning solution comprises 35% polyamide, 6% hydroxy silicone oil, 4% kaolin, and the balance is solvent, according to mass percentage. The preparation method is as follows: polyamide is added to a solvent (N-methylpyrrolidone solution) and stirred until dissolved, then hydroxy silicone oil and kaolin are added and stirred, ultrasonically dispersed at 40kHz and 40°C for 30 minutes, and finally, under the conditions of 150°C and 80% of the atmospheric pressure, the semi-cured polyamide spinning solution is obtained by vacuum distillation.
[0026] The preparation method of the graphene exothermic and hygroscopic composite yarn is as follows: modified graphene gel solution and polyamide spinning solution are placed in a high-voltage electrospinning device according to a mass ratio for core-shell double-layer spinning, and core-shell composite fiber filaments are obtained after curing (the curing treatment is well known to those skilled in the art, and this embodiment makes improvements thereto, so it is not limited thereto). The electrospinning parameters are as follows: an operating voltage of 15 kV, a receiving distance of 15 cm, a temperature of 100° C., a core layer solution advancement rate of 0.5 ml / h, and a shell layer solution advancement rate of 1 ml / h; the high-voltage electrospinning device adopts a coaxial electrospinning device, and the coaxial electrospinning device has a coaxial needle head with a double-layer structure of a shell layer needle cavity and a core layer needle cavity, the shell layer needle cavity is connected to a shell layer syringe through an injection tube, and the core layer needle cavity is connected to a core layer syringe through an injection tube, the modified graphene gel solution is used as the core layer spinning solution, and the polyamide spinning solution is used as the shell layer spinning solution.
[0027] Example 2
[0028] This embodiment provides a graphene-based heat-generating and heat-insulating fabric, which is woven from a surface fabric and a base fabric, wherein the surface fabric is woven using far-infrared fibers as warp and weft threads, and the base fabric is woven using graphene heat-generating and moisture-absorbing composite yarns as warp and weft threads;
[0029] The graphene exothermic and hygroscopic composite yarn is a core-shell composite fiber yarn obtained by core-shell double-layer electrospinning of modified graphene gel solution and polyamide spinning solution, and the mass ratio of the modified graphene gel solution to the polyamide spinning solution is 2:6.
[0030] The composition, proportion and preparation method of the far-infrared fiber are the same as those in Example 1.
[0031] The preparation method of the modified graphene gel solution is the same as that of Example 1. The polyamide spinning solution includes 45% polyamide, 6% hydroxy silicone oil, 2% kaolin, and the balance is solvent, calculated by mass percentage. The preparation method of the polyamide spinning solution is the same as that of Example 1.
[0032] The preparation method of the graphene exothermic and hygroscopic composite yarn is the same as Example 1 except that the electrospinning parameters are: the working voltage is 20 kV, the receiving distance is 12 cm, the temperature is 110° C., the core layer solution advancing rate is 1 ml / h, and the shell layer solution advancing rate is 2 ml / h.
[0033] Example 3
[0034] This embodiment provides a graphene-based heat-generating and heat-insulating fabric, which is woven from a surface fabric and a base fabric, wherein the surface fabric is woven using far-infrared fibers as warp and weft threads, and the base fabric is woven using graphene heat-generating and moisture-absorbing composite yarns as warp and weft threads;
[0035] The graphene exothermic and hygroscopic composite yarn is a core-shell composite fiber yarn obtained by core-shell double-layer electrospinning of modified graphene gel solution and polyamide spinning solution, and the mass ratio of the modified graphene gel solution to the polyamide spinning solution is 2:5.
[0036] The composition, proportion and preparation method of the far-infrared fiber are the same as those in Example 1.
[0037] The preparation method of the modified graphene gel solution is the same as that of Example 1. The polyamide spinning solution includes 40% polyamide, 10% hydroxy silicone oil, 2% kaolin, and the remainder is solvent in terms of mass percentage. The preparation method of the polyamide spinning solution is the same as that of Example 1.
[0038] The preparation method of the graphene exothermic and hygroscopic composite yarn is the same as that of Example 1.
[0039] Comparative Example 1
[0040] The difference from Example 1 is that the base fabric is obtained by weaving graphene exothermic and hygroscopic composite yarn as warp and weft; the graphene exothermic and hygroscopic composite yarn is a fiber obtained by electrostatic spinning and curing modified graphene gel liquid as raw material. The composition, ratio and preparation method of the modified graphene gel liquid are the same as those of Example 1, and the parameters of electrostatic spinning are the same as those of Example 1.
[0041] Comparative Example 2
[0042] Different from Example 1, the base fabric is obtained by weaving graphene exothermic and hygroscopic composite yarn as warp and weft threads; when preparing the graphene exothermic and hygroscopic composite yarn, modified graphene gel liquid is used as shell layer spinning liquid, and polyamide spinning liquid is used as core layer spinning liquid, the composition, ratio and preparation method of the modified graphene gel liquid are the same as those in Example 1, and the composition, ratio and preparation method of the polyamide spinning liquid are the same as those in Example 1.
[0043] In addition, a fabric obtained by weaving commercially available graphene in-situ polymerized polyamide fiber as a base fabric with the fabric disclosed in Example 1 was used as a control group.
[0044] The fabrics prepared in Example 1, Comparative 1-2 and the control group were subjected to the test according to GB / T29866-2013 "Test Method for Hygroscopic and Heat-generating Performance of Textiles". The sewn fabric samples were placed in a blast drying oven. After drying, they were moved into a drying dish for cooling. The drying dish was then placed in a constant temperature and humidity chamber for balance. A temperature sensor was inserted into the sample bag. The temperature data was recorded every 30 seconds, and the measurement time was 30 minutes. After the test, the average temperature rise value and the maximum temperature rise value of the test group and the blank control group were calculated;
[0045] The far-infrared performance of knitted fabric samples was tested in accordance with GB / T30127-2013 "Testing and Evaluation of Far-Infrared Performance of Textiles", and the far-infrared wavelength range is 8-15μm.
[0046] The results are shown in Table 1.
[0047] Table 1. Result statistics
[0048]
[0049] It can be seen from Table 1 that the fabrics prepared in Example 1, Comparative Examples 1-2 and the control group all have good far-infrared heating properties. Compared with Comparative Example 1 and the control group, Example 1 shows that the core-shell composite structure of the graphene exothermic and hygroscopic composite yarn used in Example 1 has advantages over the single-layer yarn structure in improving the hygroscopic and heating properties of the fabric. In addition, by comparing Example 1 with Comparative Example 2, it can be seen that whether the modified graphene gel liquid is used as the core layer spinning liquid or the shell layer spinning liquid, that is, the graphene material is located in the shell layer or the core layer of the composite fiber, the fabric can have good heating properties.
[0050] In order to further explore the effect of the preparation of modified graphene gel solution on the performance of fabrics, the following comparative examples were further set up:
[0051] Comparative Example 3
[0052] The only difference between this comparative example and Example 1 is that when preparing the modified graphene gel, the modified graphene used is graphene dispersed in an aqueous solution (in this embodiment, the mass volume ratio of graphene to water is 1g:10ml), and the modified graphene is separated after a rotational friction treatment for 30 minutes at a load of 100N and a rotation speed of 10r / s.
[0053] Comparative Example 4
[0054] Comparative Example The only difference between this comparative example and Example 1 is that when preparing the modified graphene gel, the modified graphene used is obtained by dispersing graphene in a p-hydroxycinnamic acid solution and stirring for 30 minutes before separation.
[0055] Comparative Example 5
[0056] The only difference between this comparative example and Example 1 is that when preparing the modified graphene gel, graphene without any modification treatment is used.
[0057] Comparative Example 6
[0058] The only difference between this comparative example and Example 1 is that when preparing the modified graphene gel, the modified graphene used is graphene dispersed in a salicylic acid solution (in this example, the mass volume ratio of graphene to salicylic acid is 1g:10ml), and the modified graphene is separated after a rotational friction treatment for 30 minutes at a load of 100N and a rotation speed of 10r / s.
[0059] Comparative Example 7
[0060] The only difference between this comparative example and Example 1 is that when preparing the modified graphene gel, the modified graphene used is graphene dispersed in a gallic acid solution (in this embodiment, the mass volume ratio of graphene to gallic acid is 1g:10ml), and the modified graphene is separated after a rotational friction treatment for 30 minutes at a load of 100N and a rotation speed of 10r / s.
[0061] Comparative Example 8
[0062] The only difference between this comparative example and Example 1 is that when preparing the modified graphene gel, the mass ratio of the modified graphene to the polypyrrole gel is 3:1.
[0063] For the fabrics prepared in Example 1 and Comparative Examples 1-8, refer to GB / T29866-2013 "Test Method for Hygroscopic Heat Performance of Textiles", and put the sewn fabric samples into a blast drying oven. After drying, move them into a drying dish for cooling. Then place the drying dish in a constant temperature and humidity chamber for balance. Insert a temperature sensor into the sample bag. Record the temperature data every 30 seconds, and the measurement time is 30 minutes. After the test, calculate the average temperature rise value and the maximum temperature rise value of the test group and the blank control group, and the results are shown in Table 2.
[0064] Table 2. Result statistics
[0065]
[0066]
[0067] As can be seen from Table 2, the fabrics prepared by Example 1 and Comparative Examples 2 and 6-7 have better hygroscopic and heat-generating properties than other comparative examples. The three are similar in that they all use acid-treated graphene. The hydrophilicity of the graphene oxide obtained after the graphene is treated with acid is enhanced, and the fabric can be prepared by adsorbing water molecules to further improve the hygroscopic and heat-generating properties of the fabric. The difference between Comparative Example 4 and Example 1 is that the graphene is not treated with rotary friction. From the data results, the heat-generating properties of the fabric are reduced. The graphene can be relatively modified in its sheet morphology and its dispersibility after rotary friction treatment, so that it can be dispersed more evenly in the modified graphene gel solution prepared later, so that its own heat-generating properties can be fully utilized, thereby improving the heat-generating properties of the fabric. Finally, the difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not contain a shell layer prepared by polyamide spinning solution. From the data results, the hygroscopic and heat-generating properties of the fabric are not as good as those of Example 1. It can be seen that the shell layer prepared by polyamide spinning solution also affects the hygroscopic and heat-generating properties of the fabric to a certain extent.
[0068] 2. The fabrics prepared in Example 1 and Comparative Examples 1-8 were based on GB / T 20944.2-2007 "Evaluation of Antibacterial Properties of Textiles" Part 2: Absorption Method, test bacteria: Staphylococcus aureus ATCC No. 6538 (Gram-positive bacteria), Escherichia coli 8099 (Gram-negative bacteria). According to the standard, the standard cloth, Example 1 and Comparative Examples 1-6 were cut into 18 mm × 18 mm sizes, and antibacterial tests were carried out after 0 and 50 washes. The results are shown in Table 3.
[0069] Table 3. Result statistics
[0070]
[0071]
[0072] It can be seen from Table 3 that Example 1 has a better antibacterial effect than other comparative examples. When p-hydroxycinnamic acid is used to treat graphene powder, p-hydroxycinnamic acid is an acid agent, which improves the antibacterial effect. Second, a π-π conjugated interaction is formed between the phenolic hydroxyl group and graphene in the p-hydroxycinnamic acid molecule, thereby adsorbing on the surface of graphene as a stabilizer to avoid its agglomeration and improve its dispersibility, resulting in a more uniform dispersion of the modified graphene in the modified graphene gel solution.
[0073] In addition, by comparing Example 1 with Comparative Example 2, it can be seen that the antibacterial effects of the two are equivalent when washed 0 times, while the antibacterial property of Comparative Example 6 after washing 50 times significantly reduces that of Example 1. The difference between Comparative Example 2 and Example 1 is that Comparative Example 6 does not contain a shell layer prepared by polyamide spinning solution. It can be seen that the shell layer prepared by polyamide spinning solution also affects the antibacterial performance of the fabric to a certain extent.
[0074] 3. The core-shell composite fiber filaments prepared in Example 1 and Comparative Examples 1-8 were tested for tensile properties of the single filaments using an Instron 6800 universal material testing machine according to GB / T 14344-2008 “Test Method for Tensile Properties of Chemical Fiber Filaments”. The results are shown in Table 3.
[0075] Table 4. Result statistics
[0076]
[0077]
[0078] From the results in Table 4, it can be seen that the tensile strength of the core layer fiber filaments prepared in Example 1 is greatly improved compared with other comparative examples. First, compared with Comparative Examples 6-7, it can be seen that the tensile strength of the core layer fiber filaments prepared in Example 1 is stronger. It can be seen that although p-hydroxycinnamic acid, salicylic acid and gallic acid can enhance the dispersibility of graphene and improve the heating performance and antibacterial performance of the fabric, salicylic acid and gallic acid have an adverse effect on the strength of the fiber filaments, which is reflected in the fact that the tensile strength of the core layer fiber filaments is not as good as that of Example 1;
[0079] Finally, by comparing Comparative Examples 3-4 with Example 1, it can be seen that the rotational friction treatment of graphene alone does not significantly improve the tensile strength of the core layer fiber filaments, but when combined with acid treatment, the tensile strength of the core layer fiber filaments is more significantly improved.
[0080] The above description shows and describes several preferred embodiments of the invention, but as mentioned above, it should be understood that the invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. Changes and modifications made by those skilled in the art should be within the scope of protection of the claims attached to the invention without departing from the spirit and scope of the invention.
Claims
1. A graphene-based heat-generating and heat-insulating fabric, characterized in that: It is woven from a surface cloth and a base cloth, wherein the surface cloth is woven with far-infrared fibers as warp and weft, and the base cloth is woven with graphene heat-generating and moisture-absorbing composite yarns as warp and weft; The graphene exothermic and hygroscopic composite yarn is a core-shell composite fiber yarn obtained by core-shell double-layer electrospinning of modified graphene gel solution and polyamide spinning solution, and the mass ratio of the modified graphene gel solution to the polyamide spinning solution is 2:4-6.
2. The graphene-based heat-generating and heat-insulating fabric according to claim 1, characterized in that: The preparation method of the modified graphene gel solution comprises the following steps: (1) dispersing graphene in a p-hydroxycinnamic acid solution, and separating and obtaining modified graphene after a rotational friction treatment for 30-60 minutes; (2) adding the modified graphene and boric acid into the polypyrrole gel and uniformly dispersing them by ultrasonication, then adding distilled water and continuously ultrasonicating until a slurry is formed, and then distilling under reduced pressure to obtain a modified graphene gel solution.
3. The graphene-based heat-generating and heat-insulating fabric according to claim 2, characterized in that: The mass ratio of the modified graphene, boric acid and polypyrrole gel is 3:0.5:1, and the amount of distilled water added is 300% of the mass of the modified graphene.
4. The graphene-based heat-generating and heat-insulating fabric according to claim 1, characterized in that: The polyamide spinning solution comprises, by weight percentage, 35-45% polyamide, 6-10% hydroxy silicone oil, 2-4% kaolin, and the remainder is solvent.
5. The graphene-based heat-generating and heat-insulating fabric according to claim 1, characterized in that: The electrospinning adopts a coaxial electrospinning device, which has a coaxial needle with a double-layer structure of a shell layer needle cavity and a core layer needle cavity. The shell layer needle cavity is connected to the shell layer syringe through an injection tube, and the core layer needle cavity is connected to the core layer syringe through an injection tube. The modified graphene gel solution is used as the core layer spinning solution, and the polyamide spinning solution is used as the shell layer spinning solution.
6. The graphene-based heat-generating and heat-insulating fabric according to claim 1, characterized in that: The parameters of the electrospinning are: working voltage of 15-20 kV, receiving distance of 12-15 cm, temperature of 100-110° C., core layer solution advancing rate of 0.1-2 ml / h, and shell layer solution advancing rate of 0.1-3 ml / h.
7. The graphene-based heat-generating and heat-insulating fabric according to claim 1, characterized in that: The far-infrared fiber is prepared by uniformly mixing dry polyurethane slices with far-infrared ceramic powder, antistatic agent and dispersant, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch and melt-spinning to obtain the far-infrared fiber.
Citation Information
Cited By
Graphene heating garment fabric and preparation method thereof
CN119932744A
Preparation method of moisture-absorbing, heating and warm-keeping kapok fabric
CN121428719A