Flexible pressure sensor with double microstructures and preparation method thereof

By integrating porous and surface micro-protruding dual microstructures in flexible pressure sensors, combining conductive polymer composite materials and interdigital electrode assembly, the contradiction between sensitivity and response range is solved, and a flexible pressure sensor with high sensitivity and wide pressure response range is achieved , suitable for a variety of applications.

CN118992967APending Publication Date: 2024-11-22ZHENGZHOU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411092341.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing flexible pressure sensors have contradictions between sensitivity and pressure response range when improving pressure sensitive performance, and the physical and chemical properties of the materials limit their further development.

Method used

Using a dual microstructure design, conductive polymer composite materials are prepared by integrating porous structures and surface microprotrusion structures in a flexible pressure sensor, and ultrasonic treatment of polymer solution and conductive filler, combined with interdigital electrode assembly to improve pressure sensitivity performance .

Benefits of technology

It realizes the high sensitivity and wide pressure response range of the flexible pressure sensor, can detect weak and large pressures, has low hysteresis and excellent long-term use performance, and is suitable for the detection of human biological signals and Morse codes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004986931270000011
    Figure HDA0004986931270000011
  • Figure HDA0004986931270000012
    Figure HDA0004986931270000012
  • Figure HDA0004986931270000013
    Figure HDA0004986931270000013
Patent Text Reader

Abstract

The invention belongs to the technical field of conductive polymer composite materials, and particularly relates to a flexible pressure sensor with double microstructures and a preparation method of the flexible pressure sensor. The preparation method comprises the following steps: adding a polymer solution into a template with a dual microstructure to obtain a matrix with an integrated microstructure; putting the matrix into a conductive filler solution, and performing ultrasonic treatment to obtain a conductive polymer composite material; and assembling the conductive polymer composite material and the interdigital electrode to obtain the flexible pressure sensor. The flexible pressure sensor prepared by the invention has a porous and surface micro-convex dual microstructure, and has the advantages of wide pressure response range, high sensitivity, low hysteresis quality and excellent long-term use performance of more than 2000 times of compression cycle; the pressure sensor can realize small object pressure detection, human body biological signal acquisition and Morse password transmission; and meanwhile, detection and identification of the sitting posture can be realized by combining a multi-channel detection device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive polymer composite materials, and in particular relates to a flexible pressure sensor with a double microstructure and a preparation method thereof. Background Art

[0002] Flexible pressure sensors are ubiquitous in many fields such as industrial automation, healthcare, aerospace, etc., and play an increasingly important role in human life. Therefore, the requirements for the performance of flexible pressure sensors are becoming increasingly stringent. Flexible strain sensors are expected to have high sensitivity to detect weak pressures such as pulse and muscle movement; at the same time, flexible strain sensors should also have a wide pressure monitoring range to detect large pressures such as foot pressure and tire pressure. However, the contradictions between various pressure sensing properties and the physical and chemical property limitations of the materials themselves have hindered the further development of flexible pressure sensors.

[0003] The structure of flexible pressure sensors is generally divided into an electrode layer and a sensing layer. Correspondingly, the components of flexible pressure sensors are divided into substrate materials, sensing materials, and electrode materials. In recent years, researchers have done a lot of work to improve the pressure sensitivity of flexible pressure sensors by structurally designing the electrodes or sensing layers of flexible pressure sensors. However, these designs usually only enhance a certain sensing performance, so there is an urgent need for a method to comprehensively improve the pressure response performance of flexible pressure sensors. Summary of the invention

[0004] The purpose of the present invention is to provide a flexible pressure sensor with a dual microstructure and a preparation method thereof, in which a porous structure and a surface micro-protrusion structure are integrated simultaneously in a flexible pressure sensor to achieve a comprehensive improvement in its pressure sensitivity performance.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0006] A flexible pressure sensor with a dual microstructure is obtained by the following preparation method, the steps are as follows:

[0007] 1) Adding a polymer solution to a template having a dual microstructure to obtain a matrix having an integrated microstructure;

[0008] 2) placing the substrate into a conductive filler solution and ultrasonically treating the substrate to obtain a conductive polymer composite material;

[0009] 3) Assembling the conductive polymer composite material and the interdigital electrodes to obtain the flexible pressure sensor.

[0010] Furthermore, in step 1), the template with the dual microstructure is composed of a template with hemispherical depressions and sugar cubes, and the sugar cubes are placed above the template with hemispherical depressions.

[0011] The hemispherical diameter of the template with hemispherical depressions is 200-800 micrometers, and the hemispherical spacing is 40-160 micrometers. Preferably, the hemispherical diameter is 500 micrometers, and the hemispherical spacing is 100 micrometers.

[0012] The template may be a PTFE (polytetrafluoroethylene) template.

[0013] Furthermore, a polymer solution is added to a container containing a template, and then the container is placed in a vacuum to remove bubbles in the template, and then heated to completely cure the polymer solution. The polymer solution is selected from at least one of PDMS (polydimethylsiloxane) and a curing agent, Ecoflex, thermoplastic polyurethane, polyethylene-butadiene-styrene block copolymer, styrene-polyisoprene-styrene block copolymer or polyester ether elastomer.

[0014] Furthermore, the polymer solution is preferably a mixture of PDMS and a curing agent in a mass ratio of 5-20:1, and the ratio is further preferably 10:1.

[0015] Afterwards, the container filled with the polymer solution is placed in a vacuum for 2 hours to expel the bubbles inside the template, and then left to stand at 80°C for 2 hours for curing. The above time and temperature can be adjusted according to the situation as long as the corresponding effect is achieved.

[0016] When the bubbles in the template are discharged, the vacuum degree can be maintained at 0.07 MPa, and the time is preferably 2 hours. This process can also accelerate the penetration of the polymer solution into the gaps of the microstructure template.

[0017] The container may be a polymethyl methacrylate (PMMA) container.

[0018] After the polymer solution is solidified, it is taken out from the container, and the sugar cube template is removed to obtain a polymer porous sponge matrix with a surface micro-convex structure, that is, a matrix with an integrated microstructure.

[0019] Specifically, the sugar cube template can be removed by washing with warm water, generally 1-5 times, preferably 3-5 times.

[0020] Furthermore, the solute of the conductive filler solution in step 2) can be selected from at least one of CNTs, CB, graphene, MXene, metal nanowires or nanoparticles.

[0021] Preferably, the conductive filler solution in step 2) of the present invention is a solution of CNTs and / or CB, and the mass ratio of solute CNTs and CB is 0-2:0-2, and the two are not 0 at the same time.

[0022] Furthermore, the mass ratio of solute CNTs:CB can be 0:1, 1:2, 1:1, 2:1, 1:0, preferably 1:1.

[0023] When PDMS is selected as the polymer material, the solvent is preferably cyclohexane, which can achieve a good swelling effect on PDMS.

[0024] The concentration of the conductive filler solution is preferably 4-7 mg / mL, and ultrasonic swelling can be performed under ultrasonic conditions at 70° C. for 1 h.

[0025] Furthermore, the conductive polymer composite material in step 2) can be ultrasonicated again in the ethanol solution for 2 minutes to remove the conductive filler that is not firmly bonded to the surface.

[0026] Finally, the side of the conductive polymer composite material having the micro-protrusion structure is assembled face to face with the interdigital electrode.

[0027] After assembly, the resistance signal can be output by connecting the wires to the electrodes on both sides of the interdigitated electrodes.

[0028] The present invention prepares a PDMS (other existing polymer materials suitable for making flexible pressure sensors can also be used) porous sponge with surface micro-hemispherical protrusions by using a sugar cube and hemispherical groove dual template method, and then constructs a carbon black (CB) / carbon nanotube (CNTs) conductive network (other conductive materials can also be used) on the surface and inside of the porous sponge by a swelling ultrasonic method, and finally obtains a flexible pressure sensor by assembling the micro-protrusion side face to face with the interdigital electrode. The present invention simultaneously improves the sensitivity and pressure response range of the flexible pressure sensor by integrating a dual microstructure of porous and surface micro-protrusions. The flexible pressure sensor prepared by the present invention has a response range far exceeding 350kPa and a pressure range of 7.10kPa. -1 It has high sensitivity and good cyclic response performance to different pressures; it can be used to detect human biological signals and recognize Morse code; combined with multi-channel detection equipment, it can realize the recognition of different sitting postures.

[0029] Compared with the prior art, the present invention has the following advantages:

[0030] The flexible pressure sensor prepared by the present invention has a dual microstructure of porous and surface micro-protrusions. The synergistic effect of the dual microstructures enables the pressure sensor to have a wide pressure response range (over 350 kPa) and high sensitivity (7.10 kPa). -1), low hysteresis, and excellent long-term performance of more than 2000 compression cycles; the pressure sensor can realize pressure detection of small objects, human biological signal collection and Morse code transmission; at the same time, by combining with multi-channel detection equipment, it can realize sitting posture detection and recognition. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of a porous PDMS sponge having a surface micro-convex structure prepared in Example 1 of the present invention;

[0032] Figure 2 This is a surface scanning electron microscope image of the CNTs / CB / PDMS conductive porous sponge prepared in Example 1 of the present invention;

[0033] Figure 3 The stress-strain curve of a single cycle compression of a porous PDMS sponge with a surface micro-convex structure prepared in Example 1 of the present invention from 10% to 80% continuous compression, and several stress-strain curves of a conductive porous sponge in 300 cycles of compression at 80% strain;

[0034] Figure 4 Strain-current response curves of the CNTs / CB / PDMS flexible pressure sensors with a dual microstructure of porous and surface micro-protrusions prepared in Examples 1-5 of the present invention (different CNTs / CB mass ratios) and the pressure sensors obtained in Comparative Examples 1-3 (no surface microstructure, different pore structure thicknesses);

[0035] Figure 5 This is the current response curve of the CNTs / CB / PDMS conductive porous sponge prepared in Example 1 to a series of small pressures and large pressures. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0037] In the embodiment of the present invention, the carbon black (CB) used has a diameter of 30 nm and a density of 1.7 to 1.9 g / cm 3 , produced by Cabot Corporation of the United States; carbon nanotubes (CNTs): average length 30-50μm, average diameter 8-15nm, provided by Chengdu Organic Chemistry Co., Ltd. of the Chinese Academy of Sciences; PDMS (including prepolymer and curing agent): numbered Sylgard 184, purchased from Dow Corning Corporation of the United States; the template with hemispherical grooves can be obtained by reverse CNC precision machining on the PTFE plate.

[0038] Example 1

[0039] A method for preparing a flexible pressure sensor with a dual microstructure, the steps are as follows:

[0040] 1) A PTFE template with a hemispherical concave microstructure is obtained by laser etching (the hemispherical diameter is 500 microns and the hemispherical spacing is 100 microns), and then the PTFE template is placed at the bottom of a PMMA container, and a layer of sugar cubes (there is no special requirement for the size, and the present invention uses a commercially available 2cmx2cmx1cm size) is placed on the PTFE template to obtain a template with a double microstructure;

[0041] 2) Mix the PDMS prepolymer and the curing agent in a mass ratio of 10:1 to prepare a PDMS precursor solution, and then pour the evenly stirred precursor solution into a container containing a double microstructure template. Subsequently, place the container in a vacuum oven (0.07MPa) for 2 hours to remove the air inside the microstructure template and accelerate the penetration of the PDMS precursor solution into the internal gaps of the microstructure. Then place the container in an 80°C oven for 2 hours to completely cure the PDMS precursor. Finally, remove the sample from the inside of the container and the concave hemispherical microstructure template, wash it in warm water 3-5 times to remove the sugar cube template, and obtain a PDMS porous sponge with a surface micro-convex structure after drying;

[0042] 3) 0.3 g of CNTs / CB (CNTs to CB mass ratio of 1:1) was added to 50 mL of cyclohexane solution to prepare an ultrasonic solution, and then the prepared PDMS porous sponge was placed in the ultrasonic solution and swelled and ultrasonicated at a power of 70 W for 1 hour. The sample was then dried in an oven and washed in an ethanol solution for 2 minutes to remove the conductive filler that was not firmly bonded to the surface, and dried again to obtain a CNTs / CB / PDMS conductive porous sponge;

[0043] 4) Finally, the side of the conductive porous sponge with micro-protrusions is assembled face to face with the interdigital electrodes to obtain a flexible pressure sensor.

[0044] Embodiment 2-5

[0045] The specific preparation method is the same as that of Example 1, except that in step 3), the mass ratios of CNTs to CB in the ultrasonic solution are different, and Examples 2-5 are 1:0, 2:1, 1:2, and 0:1, respectively.

[0046] Comparative Example 1

[0047] The preparation process of this comparative example is basically the same as that of Example 1, except that no PTFE template is added, and the prepared PDMS porous sponge has no surface micro-convex structure.

[0048] Comparative Examples 2-3

[0049] The preparation process is the same as that of Example 1, except that the thickness of the pore structure in Example 1 is the same as the thickness of sugar cubes, which is 1 cm. In this comparative example, the thickness of the pore structure (i.e., the thickness of the sample) is reduced to 0.5 cm (Comparative Example 2) and 0.75 cm (Comparative Example 3) by cutting.

[0050] Performance Test:

[0051] 1) Micromorphology observation: The obtained PDMS porous sponge with a surface micro-convex structure (corresponding to the sponge obtained in step 2 of Example 1) and the conductive porous sponge (corresponding to the sponge obtained in step 3 of Example 1) were placed in liquid nitrogen for cooling for 1 hour, and then quickly cut and quenched in a direction perpendicular to the surface micro-convex layer, and then the cross section was subjected to gold spraying treatment, and the micromorphology of the different microstructures of the samples was observed using a scanning electron microscope (Carl Zeiss GmbH, Germany, Model EV018).

[0052] Figure 1 a is a scanning electron microscope image of the porous structure inside the PDMS porous sponge in Example 1, Figure 1 a It can be seen that after the sugar cube template is dissolved and removed, the porous structure is well preserved. The porous structure allows structural deformation to still occur under high pressure, which can broaden the pressure response range of the sensor. Figure 1 b is the surface micro-protrusion structure of the porous sponge in Example 1, and the surface micro-protrusion structure is subsequently assembled face to face with the interdigital electrode. Under a small pressure, the contact area between the hemispherical micro-protrusion and the interdigital electrode can change, resulting in a decrease in contact resistance and an increase in the sensitivity of the flexible pressure sensor. Figure 1 c shows the interface between the two structures.

[0053] Figure 2 This is a scanning electron microscope image of the PDMS conductive porous sponge. Figure 2 It can be seen from a that a dense CNTs / CB conductive layer is also attached to the pore wall inside the sample, and from Figure 2 b SEM image of the microstructure surface shows that part of the CNTs / CB is also embedded in the PDMS due to the swelling effect of cyclohexane and the high energy of ultrasound.

[0054] 2) Compression performance test: The sample in Example 1 was cut into a 1 cm × 1 cm × 1 cm cube, and a universal testing machine (UTM2203, Shenzhen Sansi Zongheng Technology Co., Ltd.) was used to perform a compression performance test on the sample in the longitudinal direction. The pressure head compressed the sample at a speed of 5 mm / min, and the testing machine could simultaneously output the stress and strain of the sample.

[0055] Figure 3a is the stress-strain curve of the PDMS porous sponge without conductive filler loading under 10-80% strain compression cycle. It can be seen from the figure that the PDMS porous sponge shows almost negligible hysteresis performance under different strains, which is due to the low hysteresis of PDMS itself and the integrity of the internal porous structure. At the same time, Figure 3 b shows several stress-strain curves of CNTs / CB / PDMS conductive porous sponge during compression cycles up to 300 times at 80% strain. It can be seen from the figure that the mechanical properties of the conductive porous sponge have hardly changed, and still show almost negligible hysteresis performance, with only a slight decrease in the maximum stress. The excellent mechanical properties provide a strong foundation for the sensor's fast response recovery time and cyclic stability under different pressures.

[0056] 3) Sensing performance test

[0057] The interdigitated electrodes were connected to an electrochemical workstation (RST5200) using wires. The electrochemical workstation was able to impart a voltage of 0.3 volts to the sample and output the real-time current changes of the sample.

[0058] Different pressures are applied to the sample through a universal testing machine, and the electrochemical workstation records the real-time current value to test the pressure sensitivity performance of the flexible pressure sensor.

[0059] from Figure 4 It can be seen from a that a pressure of 0-350 kPa was applied to Examples 1-5, and Example 1 showed the most obvious current change. The sensitivity of Example 1 was 7.10 kPa respectively. -1 (0-25kPa), 2.96kPa -1 (25-350kPa), 1.09kPa -1 (135-350 kPa). At the same time, in order to test the enhancement effect of the dual microstructure pressure sensor performance, the present invention tested the sensitivity of comparative example 1. Figure 4 b It can be seen that the maximum sensitivity of the flexible pressure sensor without surface micro-protrusion structure is only 2.32 kPa -1 , which shows that the surface micro-protrusion structure has a great enhancement effect on sensitivity. Figure 4 c is the sensitivity test of samples with different pore structure thicknesses. As the pore thickness decreases, the sensitivity also decreases. However, it is worth noting that even if the pore thickness is reduced to 5 mm, the pressure response range of the sample is still greater than 350 kPa, which indicates that the pressure response range of the flexible pressure sensor in Example 1 is much greater than 350 kPa.

[0060] Figure 5a is the current response curve of a series of small pressures in the range of 0.04-0.20 kPa for the flexible pressure sensor with a dual microstructure of porous and surface micro-protrusions in Example 1. It can be seen that due to the enhancement effect of the surface micro-protrusions on the sensitivity, the pressure sensor has clear and repeatable resolution capabilities for tiny pressures as low as 0.04 kPa. Figure 5 b is the response capability of the flexible pressure sensor of Example 1 to large strain. It can be seen that the pressure sensor responds more stably to large pressure, the signal has almost no fluctuation and is completely repeatable. This is due to the low hysteresis of PDMS itself and the strong recovery ability of the porous structure.

Claims

1. A method for preparing a flexible pressure sensor with a dual microstructure, characterized in that: Here are the steps: 1) Adding a polymer solution to a template with a dual microstructure to obtain a matrix with an integrated microstructure; 2) placing the substrate in a conductive filler solution and ultrasonically treating it to obtain a conductive polymer composite material; 3) Assembling the conductive polymer composite material and the interdigital electrodes to obtain the flexible pressure sensor.

2. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 1, characterized in that: In step 1), the template with the dual microstructure is composed of a template with hemispherical depressions and a sugar cube, and the sugar cube is placed above the template with hemispherical depressions.

3. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 2, characterized in that: The template with hemispherical depressions has a hemispherical diameter of 200-800 micrometers and a hemispherical spacing of 40-160 micrometers.

4. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 1, characterized in that: The polymer solution is added into a container with a template, and the container is placed in a vacuum to expel the bubbles inside the template, and then heated to completely solidify the polymer solution.

5. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 4, characterized in that: The polymer solution is a uniform mixture of PDMS and a curing agent in a mass ratio of 5-20:

1.

6. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 4, characterized in that: After the polymer solution is solidified, it is taken out from the container, and the sugar cube template is removed to obtain a polymer porous sponge matrix with a surface micro-convex structure.

7. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 1, characterized in that: In step 2), the conductive filler solution is a solution of CNTs and / or CB, the solvent is cyclohexane, the mass ratio of solute CNTs and CB is 0-2:0-2, and the two are not 0 at the same time.

8. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 7, characterized in that: The mass ratio of solute CNTs and CB was 1:1, the concentration of the solution was 4-7 mg / mL, and ultrasonic swelling was performed at 70W.

9. The method for preparing a flexible pressure sensor with a dual microstructure according to claim 1, characterized in that: The side of the conductive polymer composite material having the micro-protrusion structure is assembled face to face with the interdigital electrode.

10. The flexible pressure sensor obtained by any one of the preparation methods of claims 1-9.

Citation Information

Cited By

  • Pressure sensor microstructure design method based on hyperelastic contact mechanics

    CN120951481A

  • Porous composite material based on internal interface contact mechanism, preparation method thereof and flexible pressure sensor

    CN122080640A