Method for preparing NASICON type solid electrolyte material through doping modification

By using element doping and liquid phase sintering technology in NASICON type sodium ion solid electrolyte, the problems of high sintering temperature and low ionic conductivity are solved, which significantly improves the cycle life and conductivity of solid-state batteries, and achieves more efficient sodium Ion transfer and battery performance.

CN118993078APending Publication Date: 2024-11-22ZHEJIANG UNIV

Patent Information

Application Number
CN202411094490.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high sintering temperature of the existing NASICON type sodium ion solid electrolyte causes sodium and phosphorus to volatilize, forming a heterogeneous phase, limiting the cycle life of the solid-state battery and low ionic conductivity.

Method used

By combining element doping and liquid phase sintering, the grain size and grain boundaries are adjusted by adding Sc3+ and Na2SiO3, the sintering temperature is reduced, and the rhombic phase with high ionic conductivity is formed, thereby improving the density and cycling performance of the electrolyte.

Benefits of technology

It significantly improves the ion conductivity and cycle life of solid-state batteries, reduces grain boundary resistance, improves the efficiency of sodium ion transmission and the charging and discharge performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993078A_ABST
    Figure CN118993078A_ABST
Patent Text Reader

Abstract

The invention relates to a sodium ion battery technology, and aims to provide a method for preparing an NASICON type solid electrolyte material through doping modification. Comprising the following steps: carrying out wet ball milling on anhydrous sodium carbonate, ammonium dihydrogen phosphate, zirconium dioxide, silicon dioxide and scandium oxide; pre-sintering after drying and sieving, and cooling to obtain precursor powder A; continuously carrying out secondary wet ball milling with a proper amount of Na2SiO3, and drying and sieving to obtain precursor powder B; pressing the precursor powder B into a blank, embedding the blank with a proper amount of mother powder, and then carrying out sintering treatment; and cooling the solid material, polishing and ultrasonically cleaning to obtain the NASICON type solid electrolyte material. According to the invention, the technical problems of high sintering temperature, low ionic conductivity and poor cycle performance of the solid-state battery are solved by utilizing a strategy of combining element doping and liquid-phase sintering and regulating and controlling the grain size and optimizing the grain boundary; the prepared solid electrolyte has good wettability and super-stability, and the charge-discharge performance and the cycle capacity are obviously improved after the solid electrolyte is used for a solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing a NASICON type solid electrolyte material by doping modification combined with element doping and liquid phase sintering, and an application of the material in a sodium solid-state battery. Background Art

[0002] The rapid development of renewable clean energy such as solar energy and wind energy has put forward higher requirements for energy storage equipment. Among them, electrochemical energy storage systems have been widely studied and applied due to their advantages such as high energy density, high energy utilization, timely response, geographical independence, and adaptability to energy storage scenarios of various scales. For example, lithium-ion batteries (LIBs) have been successfully used in electric vehicles and electronic products such as mobile phones and computers due to their high energy density. However, due to the limited reserves of lithium resources, the cost reduction space of lithium-ion batteries is getting smaller and smaller. Therefore, for large-scale energy storage systems, sodium-ion batteries with more abundant raw material reserves, lower costs and better safety performance are more economical.

[0003] At present, sodium-ion batteries mainly use organic liquid electrolytes. However, there is a risk of leakage and combustion during battery use. Therefore, the development of solid-state sodium batteries, such as replacing organic liquid electrolytes with non-flowing, non-flammable solid electrolytes, is expected to fundamentally solve the safety problems of batteries and promote the application of sodium-ion batteries in large-scale energy storage.

[0004] Commonly used sodium ion solid electrolyte systems include polymer solid electrolytes, sulfide solid electrolytes, and oxide solid electrolytes. Among them, NASICON (Na superionic conductor) type Na 1+x Zr2Six 3-x O 12 (hereinafter referred to as NZSP) oxide solid electrolytes have broad application prospects due to their advantages such as high room temperature conductivity and wide voltage window. However, in the prior art, the preparation of NASICON-type sodium ion solid electrolytes usually adopts a high-temperature solid-phase reaction method, and its sintering temperature is often above 1200°C. Excessively high sintering temperatures will accelerate the volatilization of sodium and phosphorus, induce the formation of impurities such as zirconium dioxide, lead to increased grain resistance and the formation of sodium dendrites, and ultimately limit the cycle life of solid-state batteries.

[0005] Therefore, it is necessary to propose a new technical solution to solve the above problems. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a NASICON type solid electrolyte material by doping and modification.

[0007] To solve the technical problem, the solution of the present invention is:

[0008] A method for preparing a NASICON type solid electrolyte material by doping and modification is provided, comprising the following steps:

[0009] (1) taking anhydrous sodium carbonate, ammonium dihydrogen phosphate, zirconium dioxide, silicon dioxide and scandium oxide, mixing them thoroughly, adding an appropriate amount of solvent and performing wet ball milling; drying and sieving the ball milled mixture, pre-calcining it, and cooling it to obtain a precursor powder A;

[0010] (2) Precursor powder A is fully mixed with an appropriate amount of Na2SiO3, and then subjected to secondary wet ball milling; the secondary ball milled mixture is dried and sieved to obtain precursor powder B;

[0011] (3) The precursor powder B is pressed into a green body by a tablet press, and an appropriate amount of the precursor powder B is embedded as a mother powder, and then sintered; a solid material is obtained by sintering, and after cooling, it is polished and ultrasonically cleaned to obtain a NASICON type solid electrolyte material.

[0012] As a preferred embodiment of the present invention, in step (1), the stoichiometric ratio of anhydrous sodium carbonate, diammonium phosphate, zirconium dioxide, silicon dioxide and scandium oxide is Na:P:Zr:Si:Sc=3.74:1.1:1.6:2:0.4.

[0013] As a preferred embodiment of the present invention, in the step (1), the pre-firing temperature is 800° C., the heat preservation time is 10 hours, and the pre-firing is naturally cooled to room temperature after completion.

[0014] As a preferred embodiment of the present invention, in step (2), the mass of Na2SiO3 accounts for 0.5% to 3% of the total mass of precursor powder A.

[0015] As a preferred embodiment of the present invention, in step (1) and step (2), the solvent added during wet ball milling is anhydrous ethanol, and the time for both ball millings is at least 12 hours.

[0016] As a preferred embodiment of the present invention, in the step (3), after the blank is embedded in the center of the masterbatch, it is sintered in an air atmosphere; first, the temperature is increased to 1110-1170°C at a heating rate of 2°C / min, and then kept warm for 20 hours. After sintering, it is naturally cooled to room temperature.

[0017] As a preferred embodiment of the present invention, in the step (3), the solid electrolytic material obtained by sintering is first polished with sandpaper, then polished with a metallographic polishing agent, and finally immersed in anhydrous ethanol for ultrasonic cleaning, and dried to obtain the final product.

[0018] As a preferred embodiment of the present invention, in step (3), the blank is a thin sheet, and the finally obtained NASICON solid electrolyte material is a thin sheet product suitable for cutting.

[0019] The present invention further provides a method for applying the NASICON type solid electrolyte material prepared by the aforementioned method in preparing a sodium solid-state battery, wherein the thin sheet-shaped NASICON type solid electrolyte material is used as the electrolyte, sodium vanadium phosphate is used as the positive electrode, and the metal Na sheet is used as the negative electrode; the solid-state battery is assembled in the order of a metal negative electrode shell, a gasket, a negative electrode, a solid electrolyte, a positive electrode, and a metal positive electrode shell.

[0020] Description of the invention principle:

[0021] The existing process requires a high sintering temperature. The volatilization of Na source and P source at high temperature easily produces ZrO2 phase, and the generated NZSP is a multi-grain boundary and multi-porous material, resulting in low ionic conductivity, which affects the battery life.

[0022] The innovative approach of the present invention compared with the prior art is to prepare the solid electrolyte by a method of comprehensively adding Na2SiO3, doping Sc and liquid phase sintering, and to study the most suitable sintering temperature.

[0023] Element substitution and liquid phase sintering are important ways to increase ionic conductivity and reduce densification temperature, respectively. 3+ The element-doped NZSP solid electrolyte (hereinafter referred to as NZSSP) can stabilize the rhombohedral phase and reduce the grain boundary, so the ionic conductivity will be significantly improved. However, the NZSSP prepared at present is all solid-phase sintered. 3+ On the basis of doping, low-melting-point Na2SiO3 (melting point is 1088°C) is added to produce a liquid phase during the sintering process, which promotes the formation of a rhombic phase with higher ionic conductivity and the densification of the electrolyte, thereby achieving the effect of improving the overall ionic conductivity. The Sc-doped solid electrolyte prepared by liquid phase sintering is assembled into a solid-state battery, and its cycle performance has been greatly improved.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The preparation method proposed in the present invention utilizes a strategy combining element doping and liquid phase sintering to control the grain size and optimize the grain boundary, thereby solving the technical problems of high sintering temperature, low ion conductivity and poor cycle performance of solid-state batteries in the prior art of NASICON-type sodium ion solid electrolytes.

[0026] 2. The present invention prepares element-doped solid electrolytes by a liquid phase sintering method, forms a liquid phase during the secondary sintering process, reduces the densification sintering temperature, increases the density of the electrolyte, and reduces the grain boundary resistance.

[0027] 3. The addition of Na2SiO3 additive in the present invention increases the Si / P ratio in the electrolyte, improves the sodium ion occupancy, promotes the formation of rhombohedral phase, reduces grain resistance, improves ionic conductivity, and reduces the activation energy of sodium ion transmission.

[0028] 4. The solid electrolyte prepared by the present invention has good wettability and ultrastability, and the charge and discharge performance and cycle capacity of the prepared solid-state battery are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the XRD pattern of the sodium ion solid electrolyte with a NASICON structure prepared in Example 5 of the present invention.

[0030] Figure 2 This is a cross-sectional scanning electron microscope (SEM) photograph of the NASICON structure sodium ion solid electrolyte prepared in Example 5 of the present invention.

[0031] Figure 3 Room temperature electrochemical impedance spectroscopy (EIS) graphs of the NZSSP-x% Na2SiO3 solid electrolyte sheets prepared in Examples 1-3 of the present invention and Comparative Example 1.

[0032] Figure 4 Room temperature electrochemical impedance spectroscopy (EIS) graphs of the NZSSP-1% Na2SiO3 solid electrolyte sheets prepared in Example 2 and Examples 4-6 sintered at different temperatures;

[0033] Figure 5 Arrhenius diagrams of the solid electrolytes obtained in Example 2 and Examples 4-6;

[0034] Figure 6 It is a schematic diagram comparing the cycle performance and coulombic efficiency at a current density of 0.5C after the solid electrolytes obtained in Example 2, Example 5 and Comparative Example 1 are assembled into batteries. DETAILED DESCRIPTION

[0035] Part I Implementation of the Invention

[0036] The method for preparing NASICON type solid electrolyte material by doping modification of the present invention comprises the following steps:

[0037] (1) taking anhydrous sodium carbonate, ammonium dihydrogen phosphate, zirconium dioxide, silicon dioxide and scandium oxide, mixing them thoroughly, adding an appropriate amount of solvent and performing wet ball milling; drying and sieving the ball milled mixture, pre-calcining it, and cooling it to obtain a precursor powder A;

[0038] Among them, the stoichiometric ratio of anhydrous sodium carbonate, diammonium hydrogen phosphate, zirconium dioxide, silicon dioxide and scandium oxide is Na:P:Zr:Si:Sc=3.74:1.1:1.6:2:0.4.

[0039] On the basis of the stoichiometric ratio required for element doping, the present invention additionally introduces 10wt% of sodium source and phosphorus source to inhibit the volatilization of the sodium source and phosphorus source and the generation of impurities during high-temperature calcination. That is, the stoichiometric ratio required for simple element doping is originally Na: P: Zr: Si: Sc = 3.4: 1: 1.6: 2: 0.4.

[0040] The ball milling solvent is anhydrous ethanol, and the ball milling time is at least 12 hours. The pre-burning temperature is 800°C, the heat preservation time is 10 hours, and the pre-burning is completed and naturally cooled to room temperature.

[0041] (2) Precursor powder A is fully mixed with an appropriate amount of Na2SiO3, and then subjected to secondary wet ball milling; the secondary ball milled mixture is dried and sieved to obtain precursor powder B;

[0042] The mass of Na2SiO3 accounts for 0.5% to 3% of the total mass of the precursor powder A. The ball milling solvent is anhydrous ethanol, and the ball milling time is at least 12 hours.

[0043] (3) Precursor powder B is pressed into a green body by a tablet press, and an appropriate amount of precursor powder B is used as a mother powder. The green body is embedded in the center of the mother powder, and then sintered in an air atmosphere; first, the temperature is raised to 1110-1170°C at a heating rate of 2°C / min, and then kept warm for 20 hours. After sintering, it is naturally cooled to room temperature. The solid material is sintered, and after cooling, it is first polished with sandpaper, and then polished with a metallographic polishing agent; finally, it is immersed in anhydrous ethanol for ultrasonic cleaning, and the final product is obtained after drying, which is the NASICON type solid electrolyte material.

[0044] In this step, the blank can be selected as a thin sheet, and the NASICON solid electrolyte material finally obtained is a thin sheet product suitable for cutting.

[0045] The NASICON type solid electrolyte material prepared by the present invention can be further used to prepare a sodium solid-state battery. The example is as follows: a thin sheet of NASICON type solid electrolyte material is used as an electrolyte, sodium vanadium phosphate is used as a positive electrode, and a metal Na sheet is used as a negative electrode; a solid-state battery is assembled in the order of a metal negative electrode shell, a gasket, a negative electrode, a solid electrolyte, a positive electrode, and a metal positive electrode shell. Each layer of material can be made into a circular sheet to assemble into a circular solid battery.

[0046] The preparation method of sodium vanadium phosphate positive electrode sheet is a prior art, and reference may be made to the records in existing public documents.

[0047] The preparation process of the example is as follows: sodium vanadium phosphate powder, acetylene black and polyvinylidene fluoride are taken in a mass ratio of 8:1:1, and then mixed with N-methyl-2-pyrrolidone (NMP) to obtain a slurry. The mixed slurry is coated on aluminum foil, dried in a vacuum drying oven at 80°C for 12 hours, and cut into a circular positive electrode sheet with a diameter of 12 mm.

[0048] Part II Specific Examples and Comparative Examples

[0049] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described below in conjunction with the accompanying drawings and implementation examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0050] Example

[0051] In Examples 1-6, when preparing the NASICON solid electrolyte material, the operation steps and process parameters are all performed in accordance with the contents described in Part 1. Among them, the parameters that are different are shown in Table 1.

[0052] Table 1 Variation of raw material composition and sintering conditions in Examples 1-6

[0053] project <![CDATA[Mass percentage of Na2SiO3 in precursor powder A]]> Sintering temperature Example 1 0.5wt% 1150℃ Example 2 1wt% 1150℃ Example 3 3wt% 1150℃ Example 4 1wt% 1110℃ Example 5 1wt% 1130℃ Example 6 1wt% 1170℃

[0054] Comparative Example 1

[0055] The operating steps and main parameters in Comparative Example 1 are the same as those in the above embodiments, except that: in step (2), the precursor powder A is directly subjected to secondary wet ball milling without adding Na2SiO3; the pressed blank is embedded in the precursor powder and heated to 1150°C at a heating rate of 2°C / min and sintered for 20 hours; other conditions remain unchanged.

[0056] Comparative Example 2

[0057] In this comparative example, the sodium ion solid electrolyte was prepared by a high temperature solid phase reaction method according to the scheme recorded in the literature (Shao, Y.; Zhong, G.; Lu, Y.; Liu, L.; Zhao, C.; Zhang, Q.; Hu, Y.-S.; Yang, Y.; Chen, L.A. novel NASICON-based glass-ceramic composite electrolyte with enhanced Na-Ion conductivity. Energy Storage Mater. 23. (2019). 514-521. https: / / doi.org / 10.1016 / j.ensm.2019.04.009).

[0058] The main parameters are as follows: weigh and ball-mill the precursor powder according to the stoichiometric ratio of Na:P:Zr:Si=3:1:2:2, heat to 1000°C and pre-sinter for 12 hours, press the pre-sintered powder into a billet, and then sinter at 1150°C for 24 hours to obtain a solid electrolyte.

[0059] The room temperature ionic conductivity of the solid electrolyte described in this comparative example is 0.45×10 -3 S / cm.

[0060] Comparative Example 3

[0061] In this comparative example, reference is made to Pal, SK; Saha, R.; Kumar, GV; Omar, S. Designing High Ionic Conducting NASICON-type Na3Zr2Si2PO 12 Solid-Electrolytes for Na-Ion Batteries. J. Phys. Chem. C. 124. (2020). 9161-9169. https: / / doi.org / 10.1021 / acs.jpcc.0c00543. The method recorded in the literature uses a solid-phase reaction method to prepare sodium ion solid electrolytes.

[0062] Its main parameters are as follows: weigh and ball-mill the precursor powder according to the stoichiometric ratio of Na:P:Zr:Si:Sc=3.33:1:1.67:2:0.33, heat to 1100°C and pre-sinter for 10 hours, isostatically press the pre-sintered powder to obtain a sheet material, and sinter at 1250°C for 5 hours to obtain a solid electrolyte.

[0063] The room temperature ionic conductivity of the solid electrolyte described in this comparative example is 0.96×10 -3 S / cm.

[0064] Part III Product Testing and Result Analysis

[0065] In order to further verify the superiority of the present invention over the prior art, the inventors also conducted measurement experiments on the NZSSP solid electrolytes obtained in Examples 1-6 and the comparative example, and the specific contents are as follows:

[0066] (1) X-ray diffraction analysis of the solid electrolyte obtained in Example 5 Figure 1 ) and scanning electron microscopy ( Figure 2 ) analysis, its diffraction peak is similar to that of Na3Zr2Si2PO 12 The standard card corresponds to the standard card, and there is no impurity peak such as ZrO2. The obtained electrolyte is sintered densely and the grain boundary is blurred.

[0067] (2) The solid electrolytes prepared in Examples 1-3 and Comparative Example 1 were subjected to electrochemical impedance spectroscopy tests at room temperature. The results are as follows: Figure 3 As shown, NZSSP is the solid electrolyte prepared in Comparative Example 1, NZSSP-0.5% Na2SiO3 is the solid electrolyte prepared in Example 1, NZSSP-1% Na2SiO3 is the solid electrolyte prepared in Example 2, and NZSSP-3% Na2SiO3 is the solid electrolyte prepared in Example 3. Figure 3 It can be seen that when the addition amount of Na2SiO3 is optimized to 1%, the room temperature ionic conductivity of the solid electrolyte is the largest, reaching 1.76×10 -3 S / cm, its bulk resistance (R b ) and grain boundary resistance (R gb ) are all the minimum values ​​among Examples 1-3 and Comparative Example 1.

[0068] (3) The solid electrolytes obtained in Example 2 and Examples 4-6 were subjected to electrochemical impedance spectroscopy tests at room temperature. The results are as follows: Figure 4 As shown, NZSSP-1% NSO (800 1150) is the solid electrolyte prepared in Example 2, NZSSP-1% NSO (800 1110) is the solid electrolyte prepared in Example 4, NZSSP-1% NSO (800 1130) is the solid electrolyte prepared in Example 5, and NZSSP-1% NSO (800 1170) is the solid electrolyte prepared in Example 6. Figure 4 It can be seen that the ionic conductivity obtained by sintering at 1130℃ is the highest, which is 2.00×10 -3 S / cm, its bulk resistance (R b ) and grain boundary resistance (R gb ) are the minimum values ​​in all embodiments.

[0069] (4) The solid electrolytes obtained in Example 2 and Examples 4-6 were subjected to electrochemical impedance spectroscopy tests at 10°C, 20°C, 30°C, 40°C, 50°C, and 60°C. According to the Arrhenius formula σ t T=Aexp(-Ea / K B T), find the corresponding activation energy of Na ion transfer, and the result is as follows Figure 5 As shown, the activation energy obtained under low temperature sintering at 1130°C is the smallest, which is 0.253 eV.

[0070] (5) The solid electrolytes obtained in Example 2, Example 5 and Comparative Example 1 were moved into an inert atmosphere glove box, and sodium vanadium phosphate was used as the positive electrode and the metal Na sheet was used as the negative electrode. The batteries were assembled and packaged to obtain solid-state ion batteries. The electrochemical performance tests were performed, and the charge and discharge voltage range was 2.2-3.8V, the temperature was 25°C, and the current density was 0.5C. Figure 6 The solid electrolytes prepared in Example 2, Example 5 and Comparative Example 1 are assembled into a sodium ion battery with a cycle performance and coulomb efficiency comparison diagram at a current density of 0.5C. The first charge specific capacity of Comparative Example 1 is 101.95mAh / g, the charge specific capacity after 216 cycles is 81.98mAh / g, and the capacity retention rate drops to 80%. The first charge specific capacity of Example 2 is 107.98mAh / g, the charge specific capacity after 262 cycles is 85.65mAh / g, and the capacity retention rate drops to 80%. The first charge specific capacity of Example 5 is 103.13mAh / g, the charge specific capacity after 400 cycles is 99.18mAh / g, and the capacity retention rate is 96%. The solid electrolyte is prepared by liquid phase sintering, and the cycle performance and specific capacity are improved compared with solid phase sintering.

[0071] (6) In order to make the effect of the present invention more intuitive, the bulk resistance, grain boundary resistance and room temperature ionic conductivity of different NZSP solid electrolyte sheets prepared in different embodiments and comparative examples are summarized in Table 2.

[0072] Table 2 Impedance data of examples and comparative examples

[0073] project Volume resistance(Ω) Grain boundary resistance (Ω) Room temperature ionic conductivity (S / cm) Example 1 46.28 49.27 <![CDATA[1.46×10 -3 ]]> Example 2 40.44 39.12 <![CDATA[1.76×10 -3 <!-- 5 -->]]> Example 3 43.08 58.22 <![CDATA[1.38×10 -3 ]]> Example 4 45.07 50.35 <![CDATA[1.47×10 -3 ]]> Example 5 34.96 35.36 <![CDATA[2.00×10 -3 ]]> Example 6 44.17 55.18 <![CDATA[1.41×10 -3 ]]> Comparative Example 1 48.07 72.6 <![CDATA[1.16×10 -3 ]]> Comparative Example 2 / / <![CDATA[0.45×10 -3 ]]> Comparative Example 3 / / <![CDATA[0.96×10 -3 ]]>

[0074] In summary, the present invention combines ion doping with liquid phase sintering, reduces the densification sintering temperature, and inhibits Na volatilization. On the basis of Sc doping, Na2SiO3 is used as a sintering aid to improve the density of the doped solid electrolyte, significantly reduce the grain boundary resistance, and at the same time improve the Si / P ratio and the sodium ion occupancy, promote the formation of rhombohedral phase, reduce the body resistance, and the overall ionic conductivity is increased by more than 71.55% compared with the control example, and the cycle life is increased by more than 85.2% compared with the control example. It shows that the present invention can greatly improve the ionic conductivity of the solid electrolyte, and improve the cycle life and specific capacity of the solid-state battery. At the same time, the preparation method is simple and feasible, and is suitable for large-scale production.

[0075] It should be noted that the above embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of the present application.

Claims

1. A method for preparing NASICON type solid electrolyte material by doping modification, characterized in that: The following steps are involved: (1) taking anhydrous sodium carbonate, ammonium dihydrogen phosphate, zirconium dioxide, silicon dioxide and scandium oxide, mixing them thoroughly, adding an appropriate amount of solvent and performing wet ball milling; drying and sieving the ball milled mixture, pre-calcining it, and cooling it to obtain a precursor powder A; (2) Precursor powder A is fully mixed with an appropriate amount of Na2SiO3, and then subjected to secondary wet ball milling; the secondary ball milled mixture is dried and sieved to obtain precursor powder B; (3) Pressing the precursor powder B into a green body with a tablet press, embedding it with an appropriate amount of the precursor powder B as a mother powder, and then sintering it; The solid material is obtained by sintering, and after cooling, it is polished and ultrasonically cleaned to obtain a NASICON type solid electrolyte material.

2. The method according to claim 1, characterized in that In the step (1), the stoichiometric ratio of anhydrous sodium carbonate, diammonium hydrogen phosphate, zirconium dioxide, silicon dioxide and scandium oxide is Na:P:Zr:Si:Sc=3.74:1.1:1.6:2:0.

4.

3. The method according to claim 1, characterized in that In the step (1), the pre-firing temperature is 800° C., the heat preservation time is 10 hours, and after the pre-firing is completed, it is naturally cooled to room temperature.

4. The method according to claim 1, characterized in that: In the step (2), the mass of Na2SiO3 accounts for 0.5% to 3% of the total mass of the precursor powder A.

5. The method according to claim 1, characterized in that In the step (1) and the step (2), the solvent added during the wet ball milling is anhydrous ethanol, and the time for the two ball millings is at least 12 hours.

6. The method according to claim 1, characterized in that In the step (3), after the blank is embedded in the center of the masterbatch, it is sintered in an air atmosphere; first, the temperature is increased to 1110-1170°C at a heating rate of 2°C / min, and then the temperature is kept for 20 hours. After the sintering is completed, it is naturally cooled to room temperature.

7. The method according to claim 1, characterized in that In the step (3), the solid electrolytic material obtained by sintering is firstly polished with sandpaper, then polished with a metallographic polishing agent, and finally immersed in anhydrous ethanol for ultrasonic cleaning, and dried to obtain the final product.

8. The method according to claim 1, characterized in that In the step (3), the blank is a thin sheet, and the finally obtained NASICON solid electrolyte material is a thin sheet product suitable for cutting.

9. A method for using the NASICON solid electrolyte material prepared by the method described in any one of claims 1 to 8 in preparing a sodium solid-state battery, characterized in that: The solid-state battery is composed of thin sheet NASICON solid electrolyte material as electrolyte, sodium vanadium phosphate as positive electrode, and metal Na sheet as negative electrode. The solid-state battery is assembled in the order of metal negative electrode shell, gasket, negative electrode, solid electrolyte, positive electrode, and metal positive electrode shell.

Citation Information

Patent Citations

  • Modified sodium ion solid electrolyte ceramic material with NASICON type structure as well as preparation method and application of modified sodium ion solid electrolyte ceramic material

    CN114349494A

  • Sodium ion solid electrolyte with NASICON structure as well as preparation method and application of sodium ion solid electrolyte

    CN115832415A

  • Mixed ionic and electronic conductor for solid state battery

    US20200259211A1

  • Ceramic oxide solid-state electrolyte and preparation method therefor

    WO2023092844A1

Cited By

  • Composite solid sodium battery electrolyte and preparation method thereof

    CN122267284A

  • Composite solid-state sodium battery electrolyte and method of making same

    CN122267284B

  • Rb-doped NASICON type solid sodium-ion battery electrolyte material as well as preparation method and application of Rb-doped NASICON type solid sodium-ion battery electrolyte material