Method for producing silicon inclusion compound electrode active material and method for producing lithium ion battery

By contacting the silicon closure particles with the hydrogen fluoride solution to remove the type I silicon closure composition, the expansion problem of the active substance of the silicon closure composition electrode during charging is solved, and the performance and stability of the lithium-ion battery are improved.

CN118993079APending Publication Date: 2024-11-22TOYOTA JIDOSHA KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410560188.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-05-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, silicon closure electrode active substances have expansion problems when charging, and it is difficult to effectively remove type I silicon closures, affecting the performance of lithium-ion batteries.

Method used

By contacting the silicon inclusion particles containing the type I silicon inclusion compound and the type II silicon inclusion compound with the hydrogen fluoride solution, a part of the type I silicon inclusion compound is removed by taking advantage of the difference in the solubility of hydrogen fluoride, thereby suppressing expansion during charge and discharge. .

Benefits of technology

It effectively reduces the expansion and contraction of lithium-ion batteries during charging and discharging, improves the stability and performance of the batteries, and provides a high-efficiency silicon inclusion electrode active material manufacturing method for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004827450010000111
    Figure BDA0004827450010000111
  • Figure BDA0004827450010000131
    Figure BDA0004827450010000131
  • Figure BDA0004827450010000151
    Figure BDA0004827450010000151
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a silicon inclusion compound electrode active material and a method for manufacturing a lithium ion battery. Provided are: a method for producing a silicon inclusion compound electrode active material capable of removing at least a portion of a type I silicon inclusion compound; and a method for producing a lithium ion battery including producing such a silicon inclusion compound electrode active material. The disclosed method of manufacturing a silicon clathrate electrode active material comprises: (a) providing silicon clathrate particles containing a type I silicon clathrate and a type II silicon clathrate; and (b) bringing the silicon inclusion compound particles into contact with a hydrogen fluoride solution to remove at least a portion of the type I silicon inclusion compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for producing a silicon inclusion compound electrode active material and a method for producing a lithium ion battery. Background Art

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles is advancing. In addition, silicon is known as an electrode active material used in batteries, especially lithium-ion batteries.

[0003] Silicon electrode active materials have a large theoretical capacity and are effective for increasing the energy density of batteries. However, silicon electrode active materials have a problem of large expansion during charging. In response to this, it is known that silicon inclusion compound electrode active materials can be used as silicon electrode active materials to suppress expansion during charging.

[0004] For example, Patent Document 1 discloses a silicon inclusion compound electrode active material having a silicon inclusion compound II type crystal phase, having voids inside primary particles, and voids with pore diameters of 100 nm or less having a void content of 0.05 cc / g or more and 0.15 cc / g or less.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-158004 Summary of the invention

[0008] Problems to be solved by the invention

[0009] The types of silicon clathrate crystals include type I silicon clathrate and type II silicon clathrate, etc. In particular, type II silicon clathrate crystals have a cage structure that can efficiently store lithium, so that the expansion and contraction during battery charge and discharge are small.

[0010] In view of such actual conditions, it is desired to develop a method for removing type I silicon clathrate from silicon clathrates containing both type I silicon clathrates and type II silicon clathrates.

[0011] An object of the present disclosure is to provide a method for producing a silicon clathrate electrode active material capable of removing at least a portion of type I silicon clathrate, and a method for producing a lithium ion battery including producing such a silicon clathrate electrode active material.

[0012] Means for solving problems

[0013] The present inventors have found that the above-mentioned problems can be solved by the following means.

[0014] <Scheme 1>

[0015] A method for producing a silicon inclusion compound electrode active material, comprising the following steps:

[0016] (a) providing silicon clathrate particles containing type I silicon clathrate and type II silicon clathrate; and

[0017] (b) contacting the silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate.

[0018] <Scheme 2>

[0019] The method according to claim 1, wherein in step (b), the ratio of the amount of hydrogen fluoride to the mass of the silicon clathrate particles is greater than 0.0060 mol / g and less than 0.2500 mol / g.

[0020] <Scheme 3>

[0021] The method according to Scheme 1 or 2, wherein the solvent of the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.

[0022] <Scheme 4>

[0023] The method according to any one of aspects 1 to 3, wherein in the mixed solvent, a ratio of the mass of the water to the total mass of the water and the organic solvent is 30% by mass or more and 90% by mass or less.

[0024] <Scheme 5>

[0025] The method according to any one of aspects 1 to 4, wherein the silicon inclusion compound electrode active material is used as a negative electrode active material for a lithium ion battery.

[0026] <Scheme 6>

[0027] A method for producing a lithium ion battery, comprising: producing a silicon inclusion compound electrode active material by the method according to any one of schemes 1 to 5; and forming an electrode active material layer containing the silicon inclusion compound electrode active material.

[0028] Effects of the Invention

[0029] According to the method of the present disclosure for producing a silicon inclusion compound electrode active material, at least a portion of the type I silicon inclusion compound can be removed. In addition, according to the present disclosure, a method for producing a lithium ion battery including producing such a silicon inclusion compound electrode active material can be provided. DETAILED DESCRIPTION

[0030] The following is a detailed description of the embodiments of the present disclosure. However, the present disclosure is not limited to the following embodiments, and can be implemented with various modifications within the scope of the disclosed gist.

[0031] 《Method for producing silicon inclusion compound electrode active material》

[0032] The disclosed method for producing a silicon clathrate electrode active material comprises: (a) providing silicon clathrate particles containing type I silicon clathrate and type II silicon clathrate; and (b) contacting the silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate.

[0033] The inventors of the present application have found that there is a difference in solubility between type I silicon clathrate and type II silicon clathrate in hydrogen fluoride solution. That is, it is believed that since type I silicon clathrate has a high solubility in hydrogen fluoride solution, type I silicon clathrate can be removed from silicon clathrate particles containing type I silicon clathrate and type II silicon clathrate by contacting the hydrogen fluoride solution.

[0034] By removing the type I silicon clathrate that expands and contracts more than the type II silicon clathrate during battery charge and discharge, the ratio of the type II silicon clathrate is relatively increased, thereby suppressing an increase in the confinement pressure during charge and discharge.

[0035] In the present disclosure, the “electrode active material” can be used as a “positive electrode active material” or a “negative electrode active material”, and can be used as a “negative electrode active material” in particular.

[0036] <Provision of Silicon Inclusion Compound Particles>

[0037] The method of the present disclosure includes providing silicon clathrate particles containing type I silicon clathrate and type II silicon clathrate.

[0038] Such silicon clathrate particles can be produced by preparing a sodium-silicon (NaSi) alloy and removing sodium from the NaSi alloy.

[0039] Specifically, first, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy. Then, the NaSi alloy prepared in this way is heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing silicon clathrate particles. Alternatively, the NaSi alloy prepared in this way is reacted with aluminum fluoride as a sodium scavenger to remove sodium from the NaSi alloy and form a clathrate, thereby preparing silicon clathrate particles.

[0040] <Removal of Type I Silicon Inclusion Compounds>

[0041] The method disclosed herein comprises: contacting silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of type I silicon clathrate.

[0042] In the method disclosed herein, the ratio of the amount of hydrogen fluoride in the hydrogen fluoride solution (mol) to the mass of the silicon inclusion compound particles (g) (HF [mol] / Si [g]) is preferably 0.006 mol / g or more and 0.25 mol / g or less. The ratio may be 0.01 mol / g or more, 0.02 mol / g or more, 0.03 mol / g or more, 0.04 mol / g or more, or 0.05 mol / g or less, or 0.20 mol / g or less, or 0.15 mol / g or less, 0.13 mol / g or less, or 0.11 mol / g or less. If the ratio is within the above range, the type I silicon inclusion compound can be removed from the silicon inclusion compound particles with high selectivity.

[0043] The solvent of the hydrogen fluoride solution can be water, an organic solvent, or a mixed solvent of water and an organic solvent. When the solvent contains water, that is, when the solvent is water or a mixed solvent of water and an organic solvent, particularly when the solvent is a mixed solvent of water and an organic solvent, the generation of a by-product such as sodium silicofluoride (Na2SiF6) can be suppressed, and thus it is preferred.

[0044] Furthermore, when the contact is performed with a mixing operation such as stirring, bubbles will be generated if the solvent is only water, but the generation of bubbles can be suppressed if the solvent is a mixed solvent of water and an organic solvent.

[0045] In the mixed solvent, relative to the total mass of water and the organic solvent, the ratio of the mass of water can be more than 30 mass % and less than 90 mass %. In addition, this ratio can be more than 40 mass %, more than 50 mass %, more than 60 mass %, more than 70 mass %, more than 80 mass % or 85 mass %, can be less than 89 mass %, less than 88 mass %, or less than 87 mass %.

[0046] The organic solvent may be any organic solvent capable of dissolving hydrogen fluoride, and when the organic solvent is mixed with water for use, it may be any organic solvent capable of dissolving hydrogen fluoride and compatible with water. The organic solvent is preferably an alcohol, more preferably a lower alcohol, and still more preferably ethanol.

[0047] The time for contacting the silicon clathrate particles with the hydrogen fluoride solution may be 0.1 hour or longer, 0.3 hour or longer, or 0.5 hour or longer, and may be within 6 hours, within 5 hours, or within 4 hours.

[0048] The content ratio of the type I silicon clathrate and the type II silicon clathrate in the silicon clathrate particles can be calculated from, for example, the peak intensity ratio in the measurement results of X-ray diffraction (XRD).

[0049] <use>

[0050] The silicon inclusion compound electrode active material in the method disclosed in the present invention can be used as a negative electrode active material for lithium ion batteries.

[0051] 《Manufacturing method of lithium-ion battery》

[0052] The disclosed method of manufacturing a lithium ion battery includes: manufacturing a silicon clathrate electrode active material; and forming an electrode active material layer containing the silicon clathrate electrode active material.

[0053] For the method for producing the silicon clathrate electrode active material, reference can be made to the above description related to the method for producing the silicon clathrate electrode active material of the present disclosure.

[0054] The method for forming the electrode active material layer is not particularly limited, and a known method can be used. For example, when the negative electrode active material layer contains the silicon inclusion compound electrode active material disclosed in the present invention, the electrode active material layer formed on the negative electrode collector layer, i.e., the negative electrode active material layer, can be obtained by applying a slurry containing the silicon inclusion compound electrode active material to the negative electrode collector and drying it.

[0055] The method for forming the battery is not particularly limited, and a known method can be adopted. The following describes a method for producing a battery in which the negative electrode active material layer contains the silicon inclusion compound electrode active material of the present disclosure.

[0056] The manufacturing method of the battery disclosed in the present invention may include sequentially configuring a negative electrode collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer and a positive electrode collector layer in addition to manufacturing a silicon inclusion compound electrode active material and forming a negative electrode active material layer containing the silicon inclusion compound electrode active material.

[0057] 〈Negative electrode current collector layer〉

[0058] The material used for the negative electrode collector layer is not particularly limited, and any material that can be used as a negative electrode collector for a battery can be appropriately adopted, such as copper, copper alloys, and products obtained by plating or vapor-depositing copper with nickel, chromium, carbon, etc., but is not limited to these.

[0059] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0060] <Negative electrode active material layer>

[0061] The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive aid, and a binder.

[0062] (Negative electrode active material)

[0063] The negative electrode active material includes the silicon inclusion compound electrode active material disclosed in the present invention.

[0064] (Electrolytes)

[0065] The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for lithium-ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0066] Examples of sulfide solid electrolytes include sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes, but are not limited to these. Specific examples of sulfide solid electrolytes include Li2S-P2S5 (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 (Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x PS 6-x Cl x etc.; or combinations thereof, but not limited to these.

[0067] The sulfide solid electrolyte may be glass or crystallized glass (glass ceramic).

[0068] Furthermore, when the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon inclusion compound electrode active material to the solid electrolyte in the negative electrode active material layer (mass of the silicon inclusion compound electrode active material: mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0069] The electrolyte preferably contains a supporting salt and a solvent.

[0070] As supporting salts (lithium salts) of electrolytes with lithium ion conductivity, for example, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3 can be listed.

[0071] Examples of the solvent used in the electrolyte include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC); and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolyte preferably contains two or more solvents.

[0072] (Conductive additive)

[0073] The conductive additive is not particularly limited and may be, for example, VGCF (vapor grown carbon fiber), acetylene black (AB), Ketjen black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0074] (Adhesive)

[0075] The binder is not particularly limited, and may be, for example, polyvinylidene fluoride (PVdF), butadiene rubber (BR), styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0076] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0077] 〈Electrolyte layer〉

[0078] The electrolyte layer contains at least an electrolyte. In addition, the electrolyte layer may contain a binder and the like as needed in addition to the electrolyte. For the electrolyte and the binder, reference can be made to the above description related to the negative electrode active material layer of the present disclosure.

[0079] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, or preferably 0.1 to 100 μm.

[0080] <Positive electrode active material layer>

[0081] The positive electrode active material layer is a layer containing a positive electrode active material and, optionally, an electrolyte, a conductive aid, a binder, and the like.

[0082] There is no particular limitation on the material of the positive electrode active material. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, by Li 1+x Mn 2-x-y M yO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni and Zn) is a heterogeneous element substituted Li-Mn spinel, lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co and Ni), etc., but is not limited to these.

[0083] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material having lithium ion conductivity, low reactivity with the positive electrode active material and the solid electrolyte, and a coating layer that can maintain a non-flowing state even when in contact with the active material or the solid electrolyte. Specific examples of materials constituting the coating layer include Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.

[0084] The shape of the positive electrode active material may be, for example, a particle shape. The average particle size (D50) of the positive electrode active material is not particularly limited, and may be, for example, 10 nm or more, or 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material may be, for example, 50 μm or less, or 20 μm or less. The average particle size (D50) may be calculated, for example, by measurement using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0085] For the electrolyte, the conductive aid, and the binder, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.

[0086] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte (mass of the positive electrode active material:mass of the solid electrolyte) in the positive electrode active material layer is preferably 85:15 to 30:70, more preferably 80:20 to 50:50.

[0087] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0088] 〈Positive electrode collector layer〉

[0089] There is no particular limitation on the material used in the positive electrode collector layer. Materials that can be used as positive electrode collectors for batteries can be appropriately used, such as SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium and zinc, as well as products of nickel, chromium, carbon, etc. plated or vapor-deposited on these metals, but are not limited to these.

[0090] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0091] The lithium-ion battery manufactured by the method of the present disclosure may be a liquid battery containing an electrolyte as an electrolyte layer, or a solid battery containing a solid electrolyte layer as an electrolyte layer. In addition, with respect to the present disclosure, a "solid battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore, a solid battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. In addition, the solid battery of the present disclosure may be an all-solid battery, that is, a battery that uses only a solid electrolyte as an electrolyte.

[0092] The lithium ion battery manufactured by the method disclosed herein may be a primary battery or a secondary battery.

[0093] Examples of the shape of the lithium ion battery include a coin shape, a laminate shape, a cylindrical shape, and a square shape.

[0094] Example

[0095] 《Synthesis of Silicon Inclusion Compound Electrode Active Materials》

[0096] 〈Alloying〉

[0097] (Synthesis example 1)

[0098] As a silicon (Si) source, Si powder (High Purity Science, SiEPB32) was prepared. The Si powder and metallic lithium (Li) were weighed at a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and treated with hydrogen fluoride (HF) to obtain a Si powder having voids inside the primary particles, that is, a Si powder having a porous structure.

[0099] Sodium silicon (NaSi) alloy was manufactured using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. In addition, as NaH, a product previously washed with hexane was used. NaH and Si powder having a porous structure were weighed so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed using a cutting mill. The obtained mixture was heated in an argon atmosphere in a heating furnace at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0100] 〈Inclusion Formation〉

[0101] The NaSi alloy and AlF3 were weighed in such a way that the ratio of the amount of aluminum fluoride (AlF3) to the amount of NaSi alloy was 0.34, and the weighed NaSi alloy and AlF3 were mixed with a cutter to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction container, and heated in an argon atmosphere in a heating furnace at 340°C for 60 hours to obtain a reaction product containing silicon inclusion particles. The obtained reaction product was acid-washed using a mixed solvent of HNO3 and H2O in a volume ratio of 10:90 to remove by-products in the reaction product. After washing, the solid component separated by filtration was dried at 120°C for more than 3 hours to obtain a composition containing silicon inclusion particles containing type I silicon inclusions and type II silicon inclusions.

[0102] (Synthesis Examples 2 to 5)

[0103] Compositions containing silicon clathrate particles of Synthesis Examples 2 to 5 were obtained in the same manner as in Synthesis Example 1 except that the production conditions in the clathrate formation were as shown in Table 1.

[0104] The content ratio of each component in the composition containing silicon inclusion particles of each synthesis example, and the ratio of the mass of the type II silicon inclusion to the total mass of the type I silicon inclusion and the type II silicon inclusion are shown in Table 1. In addition, the ratio of the contained components is calculated from the peak intensity ratio in the XRD measurement results. In addition, in Table 1 and Tables 2 and 3 described later, "Type II" represents the type II silicon inclusion, and "Type I" represents the type I silicon inclusion.

[0105]

Table 1

[0106]

[0107] <Removal of Type I Silicon Inclusion Compounds>

[0108] (Example 1)

[0109] For 2.2 g of the composition containing silicon inclusion particles of Synthesis Example 1, 75 ml of ion exchange water and 20 ml of ethanol were added and stirred in such a way that the mass of water was 86.7% by mass relative to the total mass of water and ethanol. A 46 wt% HF aqueous solution was added thereto so that HF ​​[mol] / Si [g] became 0.0055 mol / g. The solution was stirred for 0.5 hours to react and remove the type I silicon inclusion compound. The obtained reaction solution was filtered, and the solid component separated by filtration was washed 3 times with 50 ml of ion exchange water and then washed once with 20 ml of ethanol. After washing, it was dried at 120 ° C for one night to obtain the silicon inclusion compound electrode active material of Example 1.

[0110] (Examples 2 to 8)

[0111] Except that the conditions for removing the type I silicon inclusion compound were as described in Table 2, the same operation as in Example 1 was carried out to obtain silicon inclusion compound electrode active materials of Examples 2 to 8.

[0112] The results of Examples 1 to 8 are shown in Table 2 for the yield of the type I silicon inclusion compound removal step, the content ratio of each component in the silicon inclusion compound electrode active material, and the ratio of the mass of the type II silicon inclusion compound to the total mass of the type I silicon inclusion compound and the type II silicon inclusion compound. In Table 2 and Table 3 described below, "Si" represents a composition containing silicon inclusion compound particles.

[0113]

Table 2

[0114]

[0115] As shown in Examples 1 to 3 in Table 2, the content ratio of type I silicon inclusion complexes decreased after the type I silicon inclusion complex removal step. According to the methods of Examples 2 and 3 in which HF [mol] / Si [g] was set to 0.0545 mol / g and 0.1091 mol / g, respectively, type I silicon inclusion complexes could be removed with high selectivity.

[0116] As shown in Examples 4 to 6 in Table 2, even if the stirring time in the step of removing the type I silicon inclusion compound is different, the type I silicon inclusion compound can be removed with high selectivity.

[0117] As shown in Examples 7 and 8 in Table 2, when the type I silicon clathrate was removed using a composition containing silicon clathrate particles having a small proportion of the type I silicon clathrate, the type I silicon clathrate could be completely removed.

[0118] (Example 9)

[0119] For 2.2g of the composition containing silicon inclusion particles, 100ml of ethanol was added and stirred. A 46wt% HF aqueous solution was added thereto so that HF[mol] / Si[g] became 0.0449mol / g. The solution was stirred for 3 hours to react and remove the type I silicon inclusion. The obtained reaction solution was filtered and the solid component separated by filtration was washed 8 times with 25ml of ethanol. After washing, it was dried at 60°C overnight to obtain the silicon inclusion electrode active material of Example 9.

[0120] (Example 10)

[0121] The silicon inclusion compound electrode active material of Example 10 was obtained in the same manner as in Example 9 except that the conditions for removing the type I silicon inclusion compound were changed as described in Table 3.

[0122]

Table 3

[0123]

[0124] As shown in Table 3, the type I silicon inclusion complex can be removed with high selectivity in the method of Example 9. However, it is considered that the proportion of Na2SiF6 as a by-product is large because the solvent in the step of removing the type I silicon inclusion complex is only ethanol.

[0125] In the method of Example 10, the type I silicon inclusion complex can be removed. However, it is believed that since HF [mol] / Si [g] is large and the stirring time of the type I silicon inclusion complex removal step is too long, not only the type I silicon inclusion complex is dissolved, but also the type II silicon inclusion complex is dissolved, the yield is low, and the proportion of the type II silicon inclusion complex is small. In addition, it is believed that since the solvent in this step is only ethanol, the proportion of Na2SiF6 as a by-product is large.

Claims

1. A method for producing a silicon inclusion compound electrode active material, comprising the following steps: (a) providing silicon clathrate particles containing type I silicon clathrate and type II silicon clathrate; and (b) contacting the silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate.

2. The method according to claim 1, wherein: In the step (b), the ratio of the amount of the hydrogen fluoride to the mass of the silicon clathrate particles is greater than 0.0060 mol / g and less than 0.2500 mol / g.

3. The method according to claim 1, wherein: The solvent of the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.

4. The method according to claim 1, wherein: In the mixed solvent, a ratio of the mass of the water to the total mass of the water and the organic solvent is 30 mass % or more and 90 mass % or less.

5. The method according to claim 1, wherein: The silicon inclusion compound electrode active material is used as a negative electrode active material of a lithium ion battery.

6. A method for manufacturing a lithium-ion battery, comprising: A method according to any one of claims 1 to 5 for producing a silicon inclusion compound electrode active material; and forming an electrode active material layer containing the silicon inclusion compound electrode active material.

Citation Information

Patent Citations

  • Novel porous silicon and a preparation method thereof

    CN102400217A

  • Rapid reduction of sodium occupancy in type ii silicon clathrate by chemical etching

    US20150376016A1

  • Method for producing purified silicon fine particles

    WO2021049557A1