Preparation method of rectangular yttrium oxide with low chlorine content

Through multi-step treatments such as cycloalkane acid, liquid alkali, acetic acid and adipic acid, a rectangular yttrium oxide with low chlorine content was successfully prepared, which solved the problems of high chlorine content and irregular shape of existing yttrium oxide products, and achieved high purity and rectangularity Preparation of yttrium oxide in shape, suitable for the electronics industry.

CN118993128AActive Publication Date: 2024-11-22GUANGZHOU JIANFENG MINMETALS RARE EARTH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411087629.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing yttrium oxide products have high chlorine content and irregular particle shapes, which cannot meet the high purity and shape requirements of low chlorine content rectangular yttrium oxide in electronic consumer goods and other industries.

Method used

The cycloalkane acid solution is used to react with liquid alkali saponification, add high-purity yttrium chloride solution and stir, then use a mixed solution of acetic acid and adipic acid to back-extract, and then synthesis and filtration through ultrasonic, and finally heat up and calcined in a muffle furnace, through multiple steps The treatment yielded a rectangular yttrium oxide with low chlorine content.

Benefits of technology

The chlorine content of yttrium oxide is achieved with a chlorine content of less than 30ppm, a purity of more than 99.99%, and a rectangular particle shape, which is suitable for the electronics industry, with low process energy consumption and easy operation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of rectangular yttrium oxide with low chlorine content, which comprises the following steps: S1, adding a naphthenic acid solution into a reaction container, and adding liquid caustic soda for reaction to obtain a reaction solution; s2, adding a high-purity yttrium chloride solution into the reaction solution obtained in the step S1, discharging a water phase, and washing naphthenic acid with pure water; s3, adding a prepared mixed solution of acetic acid and adipic acid into the naphthenic acid washed in the step S2; s4, adding an oxalic acid aqueous solution into ammonia water to obtain a mixed solution; s5, adding the mixed solution obtained in the step S4 into ultrasonic synthesis equipment, then adding the mixed solution into the yttrium acetate and yttrium adipate solution obtained in the step S3, completely reacting, and filtering by adopting filter paper; s6, separating the slurry obtained by the reaction in the step S5; and S7, putting the yttrium oxalate obtained in the step S6 into a crucible, and roasting to obtain the rectangular high-purity yttrium oxide. The chlorine content of the yttrium oxide prepared by the method is lower than 30ppm, the purity of the yttrium oxide is higher than 99.99%, and the yttrium oxide is wide in application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of yttrium oxide preparation, and in particular to a method for preparing rectangular yttrium oxide with low chlorine content. Background Art

[0002] Yttrium oxide (Yttrium Oxide, chemical formula Y2O3) is an important inorganic compound and one of the rare earth oxides. Yttrium oxide is a white powder with a melting point of about 2410℃, high heat resistance and good chemical stability. In its natural state, it exists in the form of mineral yttrium ore. As an alkaline earth metal oxide, yttrium oxide exhibits alkalinity and can react with strong acids to produce salts and water. It can directly react with a variety of non-metals at high temperatures. Yttrium oxide is mainly used in the following aspects:

[0003] 1. Luminescent materials: Yttrium oxide can be used as a matrix material to form phosphors with other rare earth elements (such as europium and neodymium), which are widely used in the field of lighting, such as phosphors in LED lamps, televisions and computer screens.

[0004] 2. Ceramic materials: Due to its excellent thermal stability and mechanical properties, yttrium oxide is used as an additive for advanced ceramics, especially for the production of high-performance ceramic capacitors, oxygen sensors and high-temperature resistant ceramic parts.

[0005] 3. Optical applications: Yttrium oxide crystals have excellent optical properties and can be used as laser materials, such as the active medium in yttrium aluminum garnet (YAG) lasers.

[0006] 4. Catalyst: In the chemical industry, yttrium oxide is used as a catalyst or catalyst carrier in processes such as petroleum refining and organic synthesis reactions to improve catalytic efficiency and selectivity.

[0007] 5. Medical applications: Some yttrium compounds, such as yttrium-stabilized zirconia, are used to make artificial joints and dental implants because of their good biocompatibility.

[0008] 6. Nuclear energy application: Yttrium oxide can be doped into uranium dioxide fuel to form yttrium-stabilized uranium dioxide (YSU) to improve the performance and safety of nuclear fuel.

[0009] The chlorine content of ordinary yttrium oxide products is about 100-200ppm, and the particle shape of the scanning electron microscope image is disordered and amorphous. Some customers require high-purity yttrium oxide with a chlorine content of less than 30ppm and a rectangular particle shape. This low-chlorine rectangular yttrium oxide is mainly used in electronic consumer products, communications, computers and other electronic industries. It is a new rare earth material. Researching a preparation method for low-chlorine rectangular yttrium oxide has practical production application significance. Summary of the invention

[0010] In view of the deficiencies in the prior art, the present invention provides a method for preparing rectangular yttrium oxide with low chlorine content.

[0011] In order to achieve the above object, the technical solution adopted by the present invention is:

[0012] A method for preparing rectangular yttrium oxide with low chlorine content comprises the following steps:

[0013] S1: Add cyclohexane acid solution into a reaction container, then add liquid alkali to carry out saponification reaction. After the addition of liquid alkali is completed, continue the reaction for 5 minutes to obtain a reaction solution;

[0014] S2: adding high-purity yttrium chloride solution to the reaction solution obtained in step S1, stirring for 20 minutes, releasing the water phase, and washing the cyclopentane acid with pure water until the drainage conductivity is less than 30S / m;

[0015] S3: adding the prepared mixed solution of acetic acid and adipic acid to the cyclohexane acid washed in step S2, stirring and stripping the cyclohexane acid for 30 minutes, stripping to separate yttrium acetate and yttrium adipate solution, wherein the molar concentration of yttrium acetate is 0.2-0.4 mol / L, the molar concentration of yttrium diacetate is 0-0.03 mol / L, and the chlorine content is less than 30 ppm;

[0016] S4: adding the oxalic acid aqueous solution to the ammonia water, stirring continuously until the pH value of the solution is 6-8, and filtering to obtain a mixed solution;

[0017] S5: adding the mixed solution obtained in step S4 to an ultrasonic synthesis device, and then adding it to the yttrium acetate and yttrium adipate solutions obtained in step S3, stirring for 40 to 80 minutes under the action of ultrasound, and the stirring speed is 140 to 200 r / min. After the yttrium acetate and yttrium adipate solutions are added, the reaction is complete, and the mixture is filtered with filter paper. The mother liquor after filtration is checked with a saturated oxalic acid aqueous solution to see if it is completely precipitated;.

[0018] S6: pouring the slurry obtained by the reaction in step S5 into a small centrifuge for solid-liquid separation, adding deionized water after drying the mother liquor, turning on the centrifuge for water washing, and stopping the water washing when the conductivity of the water thrown out by the centrifuge is less than 200S / m, turning on the centrifuge for sufficient drying, and obtaining yttrium oxalate after drying;

[0019] S7: The yttrium oxalate obtained in step S6 is loaded into a crucible, and the crucible is placed in a muffle furnace. The muffle furnace is heated from room temperature to 850°C-920°C, the heating time is 90-120min, the insulation time is 100-150min, and the yttrium oxide powder is obtained after natural cooling. The powder is sieved through a 120-mesh standard sieve to obtain high-purity yttrium oxide with a chlorine content of less than 30ppm, a purity of more than 99.99%, and a rectangular particle shape.

[0020] Furthermore, in step S1, the cyclopentane acid solution is a mixed solution of cyclopentane acid, kerosene and octanol, the volume ratio of cyclopentane acid, kerosene and octanol is 1:1:3.5, the concentration of liquid alkali is 10.8 mol / L, and the volume ratio of liquid alkali to cyclopentane acid solution is 325:12.

[0021] Furthermore, the addition of the high-purity yttrium chloride solution in step S2, the addition of the liquid alkali solution in step S1 and the addition of the washed cyclopentane acid in step S3 are all performed by mist spraying. The spraying addition method can improve the stripping and reaction efficiency and has obvious effects.

[0022] Furthermore, the concentration of the high-purity yttrium chloride solution in step S2 is 0.5 mol / L, and the volume ratio of the high-purity yttrium chloride solution to the volume ratio of the cyclohexane acid solution in step S1 is 1:3.8.

[0023] Furthermore, in step S4, the concentration of oxalic acid is 5-8 wt %, the concentration of ammonia water is 12.0-14.0 mol / L, and the molar number of oxalic acid is 3.2 times that of yttrium chloride in step S2.

[0024] Furthermore, in the step S3, the concentration of acetic acid in the mixed solution of acetic acid and adipic acid is 1-1.5 mol / L, and the concentration of adipic acid is 0-0.2 mol / L. Adipic acid is added to acetic acid because adipic acid has a longer carbon chain and greater polarity, and is easier to enter into the cyclohexane acid solution, resulting in better stripping effect and less loss of yttrium.

[0025] Furthermore, in step S3, the volume ratio of the washed cyclohexane acid to the mixed solution of acetic acid and adipic acid is 3:1.

[0026] Furthermore, in step S5, the ultrasonic frequency is 28 kHz.

[0027] Furthermore, in step S7, after the muffle furnace is heated to 500° C., pure oxygen is introduced for calcination, so that the generated yttrium oxide has better purity and better rectangularity.

[0028] The preparation process of the invention has low energy consumption and is easy to operate, and other pollutants are not introduced in the preparation process. The prepared yttrium oxide chloride has a content of less than 30 ppm, a purity of more than 99.99%, a high rectangularity, and is widely used. DETAILED DESCRIPTION

[0029] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0030] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0031] Example 1

[0032] A method for preparing rectangular yttrium oxide with low chlorine content comprises the following steps:

[0033] S1: Add 6.5L of cyclohexane acid solution into a reaction container, then add 240ml of 10.8mol / L liquid alkali (sodium hydroxide solution) to carry out saponification reaction. After the addition of liquid alkali is completed, continue the reaction for 5min to obtain a reaction solution;

[0034] S2: Add 1.7 L of 0.5 mol / L high-purity yttrium chloride solution to the reaction solution obtained in step S1, stir for 20 min, release the water phase, and wash the cyclopentane acid with pure water until the drainage conductivity is less than 30 S / m;

[0035] S3: adding 2.17L of a mixed solution of acetic acid and adipic acid to the cyclohexane acid washed in step S2, stirring and stripping the cyclohexane acid for 30min, stripping to separate yttrium acetate and yttrium adipic acid solutions, wherein the molar concentration of yttrium acetate is 0.37mol / L, the molar concentration of yttrium adipate is 0.01mol / L, and the chlorine content is less than 30ppm. The acetic acid concentration in the mixed solution of acetic acid and adipic acid is 1.2mol / L, and the adipic acid concentration is 0.02mol / L;

[0036] S4: adding the oxalic acid aqueous solution to the ammonia water, and stirring continuously until the pH value of the solution is 6-8, and filtering to obtain a mixed solution, wherein the oxalic acid concentration is 6wt%, the ammonia water concentration is 14mol / L, and the molar number of oxalic acid is 3.2 times that of yttrium chloride in step S2;

[0037] S5: adding the mixed solution obtained in step S4 to an ultrasonic synthesis device, and then adding it to the yttrium acetate and yttrium adipate solutions obtained in step S3, stirring for 40 to 80 minutes under the action of ultrasound, and the stirring speed is 140 to 200 r / min. After the yttrium acetate and yttrium adipate solutions are added, the reaction is complete, and the mixture is filtered with filter paper. The mother liquor after filtration is checked with a saturated oxalic acid aqueous solution to see if the precipitation is complete, and the ultrasonic frequency is 28 kHz;

[0038] S6: pouring the slurry obtained by the reaction in step S5 into a small centrifuge for solid-liquid separation, adding deionized water after drying the mother liquor, turning on the centrifuge for water washing, and stopping the water washing when the conductivity of the water thrown out by the centrifuge is less than 200S / m, turning on the centrifuge for sufficient drying, and obtaining yttrium oxalate after drying;

[0039] S7: The yttrium oxalate obtained in step S6 is loaded into a crucible, and the crucible is placed in a muffle furnace. The temperature of the muffle furnace is programmed from room temperature to 850°C-920°C, the heating time is 90-120min, the insulation time is 100-150min, and the yttrium oxide powder is obtained after natural cooling. The powder is sieved through a 120-mesh standard sieve to obtain high-purity yttrium oxide with a chlorine content of 26ppm, a purity of 99.998%, and a rectangular particle shape. After the muffle furnace is heated to 500°C, pure oxygen is introduced for calcination.

[0040] The method of adding the high-purity yttrium chloride solution in step S2, the method of adding the liquid alkali solution in step S1 and the method of adding the washed cyclopentane acid in step S3 are all to be added by mist spray.

[0041] The cyclopentane acid solution in step S1 is a mixed solution of cyclopentane acid, kerosene and octanol, and the volume ratio of cyclopentane acid, kerosene and octanol is 1:1:3.5.

[0042] Example 2

[0043] A method for preparing rectangular yttrium oxide with low chlorine content comprises the following steps:

[0044] S1: Add 6.5L of cyclohexane acid solution into a reaction container, then add 240ml of 10.8mol / L liquid alkali (sodium hydroxide solution) to carry out saponification reaction. After the addition of liquid alkali is completed, continue the reaction for 5min to obtain a reaction solution;

[0045] S2: Add 1.7 L of 0.5 mol / L high-purity yttrium chloride solution to the reaction solution obtained in step S1, stir for 20 min, release the water phase, and wash the cyclopentane acid with pure water until the drainage conductivity is less than 30 S / m;

[0046] S3: adding 2.17L of acetic acid solution to the cyclohexane acid washed in step S2, stirring and stripping the cyclohexane acid for 30min, stripping and separating yttrium acetate solution, the yttrium acetate molar concentration is 0.35mol / L, the chlorine content is less than 30ppm, and the acetic acid concentration is 1.2mol / L;

[0047] S4: adding the oxalic acid aqueous solution to the ammonia water, and stirring continuously until the pH value of the solution is 6-8, and filtering to obtain a mixed solution, wherein the oxalic acid concentration is 6wt%, the ammonia water concentration is 14mol / L, and the molar number of oxalic acid is 3.2 times that of yttrium chloride in step S2;

[0048] S5: adding the mixed solution obtained in step S4 to an ultrasonic synthesis device, and then adding it to the yttrium acetate and yttrium adipate solutions obtained in step S3, stirring for 40 to 80 minutes under the action of ultrasound, and the stirring speed is 140 to 200 r / min. After the yttrium acetate and yttrium adipate solutions are added, the reaction is complete, and the mixture is filtered with filter paper. The mother liquor after filtration is checked with a saturated oxalic acid aqueous solution to see if the precipitation is complete, and the ultrasonic frequency is 28 kHz;

[0049] S6: pouring the slurry obtained by the reaction in step S5 into a small centrifuge for solid-liquid separation, adding deionized water after drying the mother liquor, turning on the centrifuge for water washing, and stopping the water washing when the conductivity of the water thrown out by the centrifuge is less than 200S / m, turning on the centrifuge for sufficient drying, and obtaining yttrium oxalate after drying;

[0050] S7: The yttrium oxalate obtained in step S6 is loaded into a crucible, and the crucible is placed in a muffle furnace. The muffle furnace is heated from room temperature to 850°C-920°C, the heating time is 90-120min, the insulation time is 100-150min, and the yttrium oxide powder is obtained after natural cooling. The powder is sieved through a 120-mesh standard sieve to obtain high-purity yttrium oxide with a chlorine content of 28ppm, a purity of 99.996%, and a rectangular particle shape. After the muffle furnace is heated to 500°C, pure oxygen is introduced for calcination.

[0051] The method of adding the high-purity yttrium chloride solution in step S2, the method of adding the liquid alkali solution in step S1 and the method of adding the washed cyclopentane acid in step S3 are all to be added by mist spray.

[0052] The cyclopentane acid solution in step S1 is a mixed solution of cyclopentane acid, kerosene and octanol, and the volume ratio of cyclopentane acid, kerosene and octanol is 1:1:3.5.

[0053] Comparative Example 1

[0054] A method for preparing rectangular yttrium oxide with low chlorine content comprises the following steps:

[0055] S1: Add 6.5L of cyclohexane acid solution into a reaction container, then add 240ml of 10.8mol / L liquid alkali (sodium hydroxide solution) to carry out saponification reaction. After the addition of liquid alkali is completed, continue the reaction for 5min to obtain a reaction solution;

[0056] S2: Add 1.7 L of 0.5 mol / L high-purity yttrium chloride solution to the reaction solution obtained in step S1, stir for 20 min, release the water phase, and wash the cyclopentane acid with pure water until the drainage conductivity is less than 30 S / m;

[0057] S3: adding 2.17L of acetic acid solution to the cyclohexane acid washed in step S2, stirring and stripping the cyclohexane acid for 30min, stripping and separating yttrium acetate solution, the yttrium acetate molar concentration is 0.35mol / L, the chlorine content is less than 30ppm, and the acetic acid concentration is 1.2mol / L;

[0058] S4: adding the oxalic acid aqueous solution to the ammonia water, and stirring continuously until the pH value of the solution is 6-8, and filtering to obtain a mixed solution, wherein the oxalic acid concentration is 6wt%, the ammonia water concentration is 14mol / L, and the molar number of oxalic acid is 3.2 times that of yttrium chloride in step S2;

[0059] S5: adding the mixed solution obtained in step S4 to an ultrasonic synthesis device, and then adding it to the yttrium acetate and yttrium adipate solutions obtained in step S3, stirring for 40 to 80 minutes under the action of ultrasound, and the stirring speed is 140 to 200 r / min. After the yttrium acetate and yttrium adipate solutions are added, the reaction is complete, and the mixture is filtered with filter paper. The mother liquor after filtration is checked with a saturated oxalic acid aqueous solution to see if the precipitation is complete, and the ultrasonic frequency is 28 kHz;

[0060] S6: pouring the slurry obtained by the reaction in step S5 into a small centrifuge for solid-liquid separation, adding deionized water after drying the mother liquor, turning on the centrifuge for water washing, and stopping the water washing when the conductivity of the water thrown out by the centrifuge is less than 200S / m, turning on the centrifuge for sufficient drying, and obtaining yttrium oxalate after drying;

[0061] S7: The yttrium oxalate obtained in step S6 is loaded into a crucible, and the crucible is placed in a muffle furnace. The muffle furnace is heated from room temperature to 850°C-920°C, the heating time is 90-120min, the heat preservation time is 100-150min, and the yttrium oxide powder is obtained after natural cooling. The powder is sieved through a 120-mesh standard sieve to obtain high-purity yttrium oxide with a chlorine content of 31ppm, a purity of 99.991%, and a rectangular particle shape.

[0062] The method of adding the high-purity yttrium chloride solution in step S2, the method of adding the liquid alkali solution in step S1 and the method of adding the washed cyclopentane acid in step S3 are all to be added by mist spray.

[0063] The cyclopentane acid solution in step S1 is a mixed solution of cyclopentane acid, kerosene and octanol, and the volume ratio of cyclopentane acid, kerosene and octanol is 1:1:3.5.

[0064] Comparative Example 2

[0065] A method for preparing rectangular yttrium oxide with low chlorine content comprises the following steps:

[0066] S1: Add 6.5L of cyclohexane acid solution into a reaction container, then add 240ml of 10.8mol / L liquid alkali (sodium hydroxide solution) to carry out saponification reaction. After the addition of liquid alkali is completed, continue the reaction for 5min to obtain a reaction solution;

[0067] S2: Add 1.7 L of 0.5 mol / L high-purity yttrium chloride solution to the reaction solution obtained in step S1, stir for 20 min, release the water phase, and wash the cyclopentane acid with pure water until the drainage conductivity is less than 30 S / m;

[0068] S3: adding 2.17L of acetic acid solution to the cyclohexane acid washed in step S2, stirring and stripping the cyclohexane acid for 30min, stripping and separating yttrium acetate solution, the yttrium acetate molar concentration is 0.35mol / L, the chlorine content is less than 30ppm, and the acetic acid concentration is 1.2mol / L;

[0069] S4: adding the oxalic acid aqueous solution to the ammonia water, and stirring continuously until the pH value of the solution is 6-8, and filtering to obtain a mixed solution wherein the oxalic acid concentration is 6wt%, the ammonia concentration is 14mol / L, and the molar number of oxalic acid is 3.2 times that of yttrium chloride in step S2;

[0070] S5: adding the mixed solution obtained in step S4 to an ultrasonic synthesis device, and then adding it to the yttrium acetate and yttrium adipate solutions obtained in step S3, stirring for 40 to 80 minutes under the action of ultrasound, and the stirring speed is 140 to 200 r / min. After the yttrium acetate and yttrium adipate solutions are added, the reaction is complete, and the mixture is filtered with filter paper. The mother liquor after filtration is checked with a saturated oxalic acid aqueous solution to see if the precipitation is complete, and the ultrasonic frequency is 28 kHz;

[0071] S6: pouring the slurry obtained by the reaction in step S5 into a small centrifuge for solid-liquid separation, adding deionized water after drying the mother liquor, turning on the centrifuge for water washing, and stopping the water washing when the conductivity of the water thrown out by the centrifuge is less than 200S / m, turning on the centrifuge for sufficient drying, and obtaining yttrium oxalate after drying;

[0072] S7: The yttrium oxalate obtained in step S6 is loaded into a crucible, and the crucible is placed in a muffle furnace. The temperature of the muffle furnace is programmed from room temperature to 850°C-920°C, the heating time is 90-120min, the insulation time is 100-150min, and the yttrium oxide powder is obtained after natural cooling. The powder is sieved through a 120-mesh standard sieve to obtain high-purity yttrium oxide with a chlorine content of 32ppm, a purity of 99.89%, and a rectangular particle shape. After the muffle furnace is heated to 500°C, pure oxygen is introduced for calcination.

[0073] The method of adding the high-purity yttrium chloride solution in step S2, the method of adding the liquid alkali solution in step S1 and the method of adding the washed cyclohexane acid in step S3 are all direct addition without spraying.

[0074] The cyclopentane acid solution in step S1 is a mixed solution of cyclopentane acid, kerosene and octanol, and the volume ratio of cyclopentane acid, kerosene and octanol is 1:1:3.5.

[0075] It can be seen from the above test data that the chlorine content of the rectangular high-purity yttrium oxide prepared in Examples 1 and 2 of the present invention is less than 30ppm, and the purity is greater than 99.99%. In Step S3 of Example 1, due to the use of a mixed solution of acetic acid and adipic acid, the effect is better, the product purity is higher, and the chlorine content is lower. In Step S7 of Comparative Example 1, pure oxygen calcination is not used, and the product quality is reduced; in Comparative Example 2, the addition method of the high-purity yttrium chloride solution in Step S2, the addition method of the liquid alkali solution in Step S1, and the addition method of the washed cyclopentane acid in Step S3 are all directly added without spraying, and the product quality is reduced.

Claims

1. A method for preparing rectangular yttrium oxide with low chlorine content, It is characterized in that The following steps are involved: S1: Add cyclohexane acid solution into a reaction container, then add liquid alkali to carry out saponification reaction. After the addition of liquid alkali is completed, continue the reaction for 5 minutes to obtain a reaction solution; S2: adding high-purity yttrium chloride solution to the reaction solution obtained in step S1, stirring for 20 minutes, releasing the water phase, and washing the cyclopentane acid with pure water until the drainage conductivity is less than 30S / m; S3: adding the prepared mixed solution of acetic acid and adipic acid to the cyclohexane acid washed in step S2, stirring and stripping the cyclohexane acid for 30 minutes, stripping to separate yttrium acetate and yttrium adipate solution, wherein the molar concentration of yttrium acetate is 0.2-0.4 mol / L, the molar concentration of yttrium diacetate is 0-0.03 mol / L, and the chlorine content is less than 30 ppm; S4: adding the oxalic acid aqueous solution to the ammonia water, stirring continuously until the pH value of the solution is 6-8, and filtering to obtain a mixed solution; S5: adding the mixed solution obtained in step S4 to an ultrasonic synthesis device, and then adding it to the yttrium acetate and yttrium adipate solutions obtained in step S3, stirring for 40 to 80 minutes under the action of ultrasound, and the stirring speed is 140 to 200 r / min. After the yttrium acetate and yttrium adipate solutions are added, the reaction is complete, and the mixture is filtered with filter paper. The mother liquor after filtration is checked with a saturated oxalic acid aqueous solution to see if it is completely precipitated; S6: pouring the slurry obtained by the reaction in step S5 into a small centrifuge for solid-liquid separation, adding deionized water after drying the mother liquor, turning on the centrifuge for water washing, and stopping the water washing when the conductivity of the water thrown out by the centrifuge is less than 200S / m, turning on the centrifuge for sufficient drying, and obtaining yttrium oxalate after drying; S7: The yttrium oxalate obtained in step S6 is loaded into a crucible, and the crucible is placed in a muffle furnace. The muffle furnace is heated from room temperature to 850°C-920°C, the heating time is 90-120min, the insulation time is 100-150min, and the yttrium oxide powder is obtained after natural cooling. The powder is sieved through a 120-mesh standard sieve to obtain high-purity yttrium oxide with a chlorine content of less than 30ppm, a purity of more than 99.99%, and a rectangular particle shape.

2. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that The cyclopentane acid solution in step S1 is a mixed solution of cyclopentane acid, kerosene and octanol, the volume ratio of cyclopentane acid, kerosene and octanol is 1:1:3.5, the concentration of liquid caustic soda is 10.8 mol / L, and the volume ratio of liquid caustic soda to cyclopentane acid solution is 325:

12.

3. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that The method of adding the high-purity yttrium chloride solution in step S2, the method of adding the liquid alkali solution in step S1 and the method of adding the washed cyclopentane acid in step S3 are all to be added by mist spray.

4. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that The concentration of the high-purity yttrium chloride solution in step S2 is 0.5 mol / L, and the volume ratio of the high-purity yttrium chloride solution to the volume ratio of the cyclohexane acid solution in step S1 is 1:3.

8.

5. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that In step S4, the concentration of oxalic acid is 5-8 wt %, the concentration of ammonia water is 12.0-14.0 mol / L, and the molar number of oxalic acid is 3.2 times that of yttrium chloride in step S2.

6. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that In the step S3, the concentration of acetic acid in the mixed solution of acetic acid and adipic acid is 1-1.5 mol / L, and the concentration of adipic acid is 0-0.2 mol / L.

7. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that The volume ratio of the washed cyclohexane acid to the mixed solution of acetic acid and adipic acid in step S3 is 3:

1.

8. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that The ultrasonic frequency in step S5 is 28 kHz.

9. The method for preparing rectangular yttrium oxide with low chlorine content according to claim 1, It is characterized in that In step S7, after the muffle furnace is heated to 500° C., pure oxygen is introduced to carry out calcination.