Tantalum-niobium-loaded organic phase precipitation reverse extraction and reverse extraction wastewater treatment method
By using the precipitation and stripping method of the organic phase supported by the tantalum niobium metallurgy process and the boron-containing liquid in the tantalum niobium metallurgy process, the problems of low stripping efficiency and ammonia nitrogen pollution are solved, and efficient tantalum niobium metallurgy process flow and production of high-purity products are achieved. .
Patent Information
- Application Number
- CN202411106439.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The existing tantalum and niobium metallurgy process has low back-extraction efficiency, high ammonia consumption and ammonia nitrogen pollution, resulting in low production efficiency and product quality decline.
Using the method of precipitation and back-extraction of tantalum niobium organic phase and treatment of the wastewater of the back-extraction of the tantalum niobium organic phase, the precipitation and fluorine-containing boron wastewater were obtained by adding boron-containing liquid to the tantalum niobium organic phase for stirring and precipitation and back-extraction, and then tantalic acid or niobium acid precipitation and fluorine-containing boron wastewater were washed , drying and calcining convert it into tantalum pentoxide or niobium pentoxide products, and at the same time, the fluoroboride wastewater is crystallized and treated with the added value to the fluoroborate by-product.
It significantly shortens the process flow, reduces the consumption of drugs, improves the treatment efficiency and element recovery rate, avoids ammonia nitrogen pollution, and improves working conditions.
Smart Images

Figure CN118993148A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rare metal hydrometallurgy, in particular to a clean metallurgical method for efficient stripping and precipitation of tantalum and niobium. Background Art
[0002] Tantalum niobium metal and its compounds play an indispensable role in electronic information, new energy, space, superconductivity, biology and other technological fields. With the vigorous development of high-tech industries, the demand for tantalum niobium products in modern society has increased dramatically.
[0003] Tantalum-niobium concentrate, waste alloy, metallurgical slag, etc. are the main raw materials for industrial extraction of tantalum-niobium. In the mainstream tantalum-niobium metallurgical process, tantalum-niobium raw materials need to go through acid dissolution, extraction, impurity removal, stripping, precipitation, calcination and other main processes to be processed into tantalum-niobium oxide powder. Among them, the acid dissolution process often uses a high concentration of hydrofluoric acid-sulfuric acid mixture as a leaching agent; the stripping process often uses a dilute sulfuric acid solution or pure water as a stripping agent; the precipitation process is to add ammonia water or liquid ammonia to increase the pH to 8-9 to achieve neutralization precipitation; for precipitation wastewater, ammonia and ammonium bifluoride are extracted by heating the evaporator.
[0004] The stripping and precipitation steps in the above process have the following deficiencies: (1) During the stripping process, the metal concentration difference between the liquid-liquid phases gradually decreases, the acidity of the water phase gradually increases, the driving force for metal separation gradually weakens, and the number of niobium or tantalum stripping stages is as high as 10 to 20, which reduces production efficiency; (2) Precipitating tantalum or niobium from the solution requires a large amount of ammonia water or liquid ammonia, causing waste gas pollution, increased wastewater, and poor working conditions; and the pH value at the ammonia precipitation endpoint is high, so some impurity metals are precipitated together with tantalum and niobium, reducing product quality.
[0005] In summary, the current mainstream tantalum-niobium metallurgical process in the industry has problems such as low stripping efficiency, large ammonia consumption and ammonia nitrogen pollution. The development of new tantalum-niobium efficient stripping and ammonia-free precipitation technology is of great practical significance to the green quality development of the tantalum-niobium industry. Summary of the invention
[0006] In view of the problems of low liquid-liquid stripping efficiency and neutralization precipitation ammonia nitrogen pollution in tantalum-niobium hydrometallurgy, the present invention provides a method for precipitation stripping of tantalum-niobium loaded organic phase and treatment of stripping wastewater, aiming to achieve efficient and clean tantalum-niobium metallurgy with a shorter process flow, and the main steps of the method include: (1) adding a boron-containing liquid to the tantalum-niobium loaded organic phase, stirring for precipitation stripping, and obtaining an organic-water-solid mixed phase; (2) separating the mixed phase to obtain tantalate or niobic acid precipitate, a blank organic phase and fluorine-boron-containing wastewater; (3) washing, drying and calcining tantalate or niobic acid to convert it into tantalum pentoxide or niobium pentoxide product; (4) crystallizing the fluorine-boron-containing wastewater to increase the value of fluoroborate byproduct.
[0007] The present invention discloses a method for precipitation stripping of a tantalum-niobium loaded organic phase and treatment of stripping wastewater. The tantalum-niobium loaded organic phase is an extraction phase of tantalum or niobium in a hydrofluoric acid solution, which is a common intermediate product in industrial processes. In the loaded organic phase, tantalum or niobium is combined with an extractant in the form of fluorine complex ions.
[0008] The present invention discloses a method for precipitation stripping of a tantalum-niobium loaded organic phase and treatment of stripping wastewater. In the precipitation stripping process, stripping and precipitation of tantalum / niobium are carried out simultaneously, and the molar ratio of boron in a boron-containing liquid to fluorine in an organic phase loaded with tantalum and niobium is regulated to be (0.20-0.35):1.0, and more preferably (0.25-0.29):1.0; the volume ratio of aqueous phase to organic phase is (0.1-3.0):1.0, and more preferably (0.25-2):1.0, and even more preferably (0.75-2):1.0.
[0009] The concentration of fluorine in the organic phase supporting tantalum and niobium is 0.5 to 7 mol / L, preferably 1 to 6 mol / L.
[0010] The concentration of tantalum in the tantalum-niobium loaded organic phase is greater than or equal to 0.1 mol / L, preferably 0.1 to 0.25 mol / L, and more preferably 0.15 to 0.25 mol / L. The technology developed by the present invention can process a tantalum-niobium loaded organic phase with a tantalum concentration of 0.1 mol / L. When the concentration of tantalum in the tantalum-niobium loaded organic phase is 0.15 to 0.25 mol / L, the effect is better.
[0011] The concentration of niobium in the organic phase loaded with tantalum and niobium is greater than or equal to 0.3 mol / L. That is, the technology developed by the present invention can process the organic phase loaded with tantalum and niobium with a niobium concentration of 0.3 mol / L. When the concentration of tantalum in the organic phase loaded with tantalum and niobium is 0.35-0.9 mol / L, the effect is better.
[0012] The present invention discloses a method for stripping of organic phase precipitation loaded with tantalum and niobium and treatment of stripping wastewater, wherein the boron-containing liquid has at least one of metaborate, boric acid and metaboric acid as solute. The solute is further preferably sodium metaborate or boric acid. In the present invention, the selection of the solute type in the boron-containing liquid has a great influence on the purity of the potassium tetrafluoroborate product.
[0013] During the mixing process of the boron-containing liquid and the tantalum-niobium loaded organic phase, due to the strong affinity between fluorine and boron ions, fluorine prefers to complex with boron, and the initial fluorine-tantalum / fluorine-niobium complex ions are destroyed; after losing the fluorine complex, tantalum and niobium can be precipitated as tantalate (i.e. tantalum oxide hydrate) and niobium acid (i.e. niobium oxide hydrate) under pH <1 conditions, so the amount of boron-containing liquid added is less than that of the traditional ammonia water / liquid ammonia neutralization precipitation system.
[0014] It is currently reported that pure water or dilute sulfuric acid is used to strip niobium or tantalum from an organic phase loaded with tantalum and niobium. The metal concentration difference between the organic phase and the aqueous phase gradually decreases, while the acidity of the aqueous phase gradually increases, resulting in insufficient chemical driving force for interphase mass transfer and a large number of stripping unit stages. In the precipitation stripping process of the present invention, the boron-containing liquid acts as a stripping agent and a precipitant at the same time. Under the synergistic effect of the complexation-precipitation reaction, tantalum / niobium is efficiently separated from the loaded organic phase with only one mixing and stirring. The present invention replaces the traditional step-by-step multi-stage stripping and ammonia neutralization and precipitation steps with an integrated stripping-precipitation, which significantly shortens the process flow; and a boron-containing liquid precipitation stripping system is constructed, which is free of ammonia nitrogen pollution and significantly improves the working conditions.
[0015] The present invention discloses a method for stripping of organic phase precipitation loaded with tantalum and niobium and treatment of stripping wastewater. The three-phase separation is to separate tantalate or niobate precipitate, blank organic phase and fluorine-boron-containing wastewater from the mixed phase formed by stripping precipitation by means of standing, liquid separation, centrifugation, sedimentation, filtration, etc. The blank organic phase contains at least one of methyl isobutyl ketone, sec-octanol, tributyl phosphate, cyclohexanone and acetamide, and the blank organic phase can be reused for front-end tantalum and niobium extraction.
[0016] The invention discloses a method for precipitation stripping of a tantalum-niobium loaded organic phase and treatment of stripping wastewater. The crystallization treatment is to prepare fluoroborate by evaporation and crystallization of fluorine-boron-containing wastewater or by adding potassium salt for precipitation.
[0017] As a preferred embodiment, when sodium metaborate solution is used as a precipitation stripping agent, the generated fluorine-boron wastewater is subjected to evaporation crystallization to prepare sodium fluoroborate, or potassium fluoroborate is prepared by adding potassium salt for precipitation crystallization; when boric acid or metaboric acid is used as a precipitation stripping agent, the fluorine-boron wastewater is subjected to precipitation crystallization by adding potassium salt to prepare potassium fluoroborate.
[0018] The present invention discloses a method for stripping of organic phase precipitation loaded with tantalum and niobium and treatment of stripping wastewater. Tantalate or niobate is washed with pure water or boron-containing liquid to elute fluorine, boron ions or impurity precipitates adsorbed on the surface of tantalum / niobate. The washed tantalate or niobate is dried and then calcined at a high temperature of 600 to 1000°C in an atmosphere containing oxygen or water vapor to be converted into tantalum pentoxide or niobium pentoxide products. The oxygen-containing atmosphere can enhance decarburization, while the water vapor-containing atmosphere can enhance defluorination.
[0019] The present invention takes the organic phase loaded with tantalum and niobium as the treatment object for the first time, introduces an appropriate amount of boron-containing liquid into the organic phase, stirs for precipitation and stripping, obtains an organic-water-solid mixed phase, and then separates the mixed phase to obtain tantalate or niobic acid precipitate, a blank organic phase and fluorine-boron-containing wastewater; the obtained tantalate or niobic acid is washed, dried, calcined, and converted into tantalum pentoxide or niobium pentoxide products; the obtained fluorine-boron wastewater is crystallized and increased in value to be a fluoroborate byproduct.
[0020] Compared with the prior art, the present invention has a short process flow, low reagent consumption, high processing efficiency, and high recovery rate of each element. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with specific examples. It should be noted that these examples are only for a better understanding of the present invention, rather than limiting the scope of protection of the present invention.
[0023] Example 1
[0024] The tantalum-loaded organic phase obtained by extraction with 2-octanol in a hydrofluoric acid-sulfuric acid system was used as the raw material. After analysis and testing, it was confirmed that the tantalum concentration in the loaded organic phase was 0.21 mol / L and the fluorine concentration was 1.37 mol / L. Sodium metaborate solution with a boron concentration of 0.49 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 0.75:1 between the aqueous phase and the organic phase, and the molar ratio of boron to fluorine in the mixed solution was 0.268; the mixed solution was stirred at 250 rpm for 40 minutes at room temperature for precipitation stripping; the mixed phase produced by precipitation stripping was allowed to stand for 6 hours, and then the surface blank organic phase (2-octanol) was recovered by separation, and then the tantalate precipitate and fluorine-containing boron wastewater were separated by filtration. For tantalate precipitation, the precipitate is washed three times with pure water, and the washed tantalate is placed in a 150°C oven for drying for 8 hours, then placed in a rotary tube furnace and heated to 900°C, and calcined in an air atmosphere for 1.5 hours to obtain the main product tantalum pentoxide; for fluorine-boron wastewater, it is heated to 160°C, the water is evaporated, and sodium tetrafluoroborate is obtained as a by-product.
[0025] The blank organic phase and fluorine-boron-containing wastewater were tested and found that the tantalum precipitation stripping recovery rate reached 99.6%. The roasting product was tested and found that the purity of tantalum pentoxide product was 99.83%. The evaporation crystallization product was tested and found that the purity of sodium tetrafluoroborate by-product was 98.9%.
[0026] Example 2
[0027] The same tantalum-loaded organic phase as in Example 1 was used as a raw material. A sodium metaborate solution having a boron concentration of 0.38 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 1:1 between the aqueous phase and the organic phase, so as to obtain a mixed solution having a boron to fluorine molar ratio of 0.277; the mixed solution was placed in a shaker, shaken at room temperature for 40 minutes, and subjected to precipitation stripping; the mixed phase produced by precipitation stripping was placed in a centrifuge, and centrifuged at 8000 rpm for 10 minutes; after centrifugation, the surface blank organic phase (sec-octanol) was first recovered by separation, and then the tantalate precipitate and the fluorine-boron-containing wastewater were separated by filtration. For tantalate acid precipitation, the precipitate is first washed once with the aforementioned sodium metaborate solution, and then washed twice with pure water. The washed tantalate is placed in a 150°C oven for drying for 8 hours, then placed in a rotary tube furnace and heated to 950°C, and calcined for 1 hour in an air atmosphere containing 10% water vapor to obtain the main product tantalum pentoxide; for fluorine-boron-containing wastewater, potassium sulfate is added in a potassium and fluorine molar ratio of 1:4, the reaction is stirred for salting out and crystallization, and potassium tetrafluoroborate by-product is obtained, and sodium sulfate is subsequently separated by evaporation and crystallization.
[0028] The blank organic phase and fluorine-boron-containing wastewater were tested and found that the tantalum precipitation stripping rate reached 99.8%. The roasting product was tested and found that the purity of tantalum pentoxide product was 99.91%. The salting-out crystallization product was tested and found that the purity of potassium tetrafluoroborate by-product was 99.2%.
[0029] Example 3
[0030] The tantalum-loaded organic phase obtained by extracting tributyl phosphate in a hydrofluoric acid-sulfuric acid system was used as the raw material. After analysis and testing, it was confirmed that the tantalum concentration in the loaded organic phase was 0.17 mol / L and the fluorine concentration was 1.05 mol / L. Boric acid solution with a boron concentration of 0.14 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 2:1 between the aqueous phase and the organic phase, and the molar ratio of boron to fluorine in the mixed solution was 0.267; the mixed solution was stirred at 300 rpm for 30 minutes at room temperature for precipitation stripping; the mixed phase produced by precipitation stripping was placed in a centrifuge and centrifuged at 9000 rpm for 10 minutes; after centrifugation, the surface blank organic phase (tributyl phosphate) was first separated and recovered, and then the tantalate precipitate and fluorine-containing boron wastewater were separated by filtration. For tantalate precipitation, pure water is used to wash the precipitate three times. The washed tantalate is placed in a 150°C oven and dried for 8 hours. It is then placed in a rotary tube furnace and heated to 850°C. It is kept warm and calcined in an air atmosphere for 2 hours to obtain the main product tantalum pentoxide. For fluorine-boron-containing wastewater, potassium carbonate is added in a potassium and fluorine molar ratio of 1:4, the reaction is stirred for salting out and crystallization, and potassium tetrafluoroborate is obtained as a by-product.
[0031] The blank organic phase and fluorine-boron-containing wastewater were tested and found that the tantalum precipitation stripping recovery rate reached 99.5%. The roasting product was tested and found that the purity of tantalum pentoxide product was 99.85%. The salting-out crystallization product was tested and found that the purity of potassium tetrafluoroborate by-product was 99.4%.
[0032] Example 4
[0033] The niobium-loaded organic phase obtained by extraction with methyl isobutyl ketone in a hydrofluoric acid-sulfuric acid system was used as the raw material. After analysis and testing, it was confirmed that the niobium concentration in the loaded organic phase was 0.86 mol / L and the fluorine concentration was 5.58 mol / L. Sodium metaborate solution with a boron concentration of 1.82 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 0.8:1 between the aqueous phase and the organic phase, and the molar ratio of boron to fluorine in the mixed solution was 0.261; the mixed solution was placed in a shaker and shaken at room temperature for 40 minutes for precipitation stripping; the mixed phase produced by precipitation stripping was allowed to stand for 8 hours, and then the surface blank organic phase (methyl isobutyl ketone) was first separated and recovered, and then the niobium acid precipitate and fluorine-containing boron wastewater were separated by filtration. For niobic acid precipitation, the precipitate is first washed once with the aforementioned sodium metaborate solution, and then washed once with pure water. The washed niobic acid is placed in a 150°C oven for drying for 8 hours, then placed in a rotary tube furnace and heated to 900°C, and calcined in an oxygen-rich air (~30% oxygen) atmosphere for 1 hour to obtain the main product niobium pentoxide; for fluorine-boron wastewater, it is heated to 160°C, the water is evaporated to dryness, and sodium tetrafluoroborate by-product is obtained.
[0034] The blank organic phase and fluorine-boron-containing wastewater were tested and found that the stripping rate of niobium precipitation reached 99.4%. The calcined product was tested and found that the purity of niobium pentoxide product was 99.92%. The evaporation crystallization product was tested and found that the purity of sodium tetrafluoroborate by-product was 99.2%.
[0035] Example 5
[0036] The niobium-loaded organic phase obtained by extracting tributyl phosphate in a hydrofluoric acid-sulfuric acid system was used as the raw material. After analysis and testing, it was confirmed that the niobium concentration in the loaded organic phase was 0.44 mol / L and the fluorine concentration was 2.76 mol / L. Boric acid solution with a boron concentration of 0.50 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 1.5:1 between the aqueous phase and the organic phase, and the molar ratio of boron to fluorine in the mixed solution was 0.272; the mixed solution was stirred at 300 rpm for 30 minutes at room temperature for precipitation stripping; the mixed phase produced by precipitation stripping was placed in a centrifuge and centrifuged at 10,000 rpm for 6 minutes; after centrifugation, the surface blank organic phase (tributyl phosphate) was first recovered by separation, and then the niobium acid precipitate and fluorine-containing boron wastewater were separated by filtration. For niobic acid precipitation, the precipitate is washed once with the aforementioned boric acid solution, and then washed twice with pure water. The washed niobium acid is placed in an oven at 180°C for 6 hours, then placed in a rotary tube furnace and heated to 900°C, and calcined in an air atmosphere for 2 hours to obtain the main product niobium pentoxide; for fluorine-boron-containing wastewater, potassium carbonate is added in a potassium and fluorine molar ratio of 1:4, the reaction is stirred for salting out and crystallization, and potassium tetrafluoroborate by-product is obtained.
[0037] The blank organic phase and fluorine-boron-containing wastewater were tested and found that the niobium precipitation stripping recovery rate reached 99.7%. The roasting product was tested and found that the purity of niobium pentoxide product was 99.87%. The salting-out crystallization product was tested and found that the purity of potassium tetrafluoroborate by-product was 99.4%.
[0038] Example 6
[0039] The same tantalum-loaded organic phase as in Example 5 was used as the raw material. A metaboric acid solution with a boron concentration of 1.05 mol / L was added to the niobium-loaded organic phase at a volume ratio of 0.75:1 between the aqueous phase and the organic phase, so that the molar ratio of boron to fluorine in the mixed solution was 0.285; the mixed solution was placed in a shaker and shaken at room temperature for 30 minutes for precipitation stripping; the mixed phase produced by precipitation stripping was allowed to stand for 8 hours, and then the surface blank organic phase (tributyl phosphate) was first recovered by liquid separation, and then the niobium acid precipitate and the fluorine-containing boron wastewater were separated by filtration. For the niobium acid precipitate, the precipitate was washed with pure water 4 times, and the washed niobium acid was placed in a 180°C oven for 6 hours, then loaded into a rotary tube furnace and heated to 950°C, and kept warm for 2 hours in an air atmosphere to obtain the main product niobium pentoxide; for the fluorine-containing boron wastewater, potassium carbonate was added at a potassium and fluorine molar ratio of 1:4, and the reaction was stirred for salting out and crystallization to obtain potassium tetrafluoroborate as a byproduct.
[0040] The blank organic phase and fluorine-boron-containing wastewater were tested and found that the niobium precipitation stripping recovery rate reached 99.8%. The roasting product was tested and found that the purity of niobium pentoxide product was 99.91%. The salting-out crystallization product was tested and found that the purity of potassium tetrafluoroborate by-product was 99.3%.
[0041] Comparative Example 1
[0042] The same tantalum-loaded organic phase as in Example 1 was used as a raw material. A sodium metaborate solution having a boron concentration of 0.22 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 0.75:1 between the aqueous phase and the organic phase, to obtain a mixed solution having a molar ratio of boron to fluorine of 0.12; the subsequent other operations were the same as in Example 1. The blank organic phase and the fluorine-boron-containing wastewater were tested to show that the tantalum precipitation stripping recovery rate was less than 60%.
[0043] In this comparative example, the amount of sodium metaborate added is small and the boron-fluorine molar ratio is low.
[0044] Comparative Example 2
[0045] The same tantalum-loaded organic phase as in Example 1 was used as a raw material. A sodium tetraborate solution having a boron concentration of 0.49 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 0.75:1 between the aqueous phase and the organic phase, to obtain a mixed solution having a molar ratio of boron to fluorine of 0.268; the subsequent other operations were the same as in Example 1. The evaporation crystal product was tested and found to have a sodium tetrafluoroborate byproduct with a purity of only 86.3%, with a large amount of boric acid impurities mixed therein.
[0046] In this comparative example, the boron-containing liquid does not use metaborate, metaboric acid or boric acid as solute.
[0047] Comparative Example 3
[0048] The same tantalum-loaded organic phase as in Example 4 was used as the raw material. A sodium metaborate solution having a boron concentration of 1.0 mol / L was added to the tantalum-loaded organic phase at a volume ratio of 4:1 between the aqueous phase and the organic phase, to obtain a boron to fluorine molar ratio of 0.717 in the mixed solution; the subsequent other operations were the same as in Example 4. The calcined product was tested to show that the purity of the niobium pentoxide product was 98.46%, with a small amount of boric acid impurities that were not washed clean; the evaporation crystallization product was tested to show that the purity of the sodium tetrafluoroborate byproduct was 64.72%, with a large amount of impurities such as sodium fluoride and boric acid mixed therein.
[0049] In this comparative example, the aqueous phase-organic phase volume ratio and the boron-fluorine molar ratio are too high, which not only increases the consumption of chemical reagents, but also significantly reduces the purity of the main product and by-products.
Claims
1. A method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater, characterized in that: Taking the organic phase loaded with tantalum and niobium as the object, a boron-containing liquid is added for precipitation and stripping, and after three-phase separation, tantalate or niobate precipitate, a blank organic phase and fluorine-boron-containing wastewater are obtained. Tantalate or niobate is washed, dried, calcined, and converted into tantalum pentoxide or niobium pentoxide products; fluorine-boron-containing wastewater is crystallized and added to become a fluoroborate byproduct; During the precipitation stripping process, stripping and precipitation of tantalum / niobium are carried out simultaneously, and the molar ratio of boron in the boron-containing liquid and fluorine in the tantalum-niobium loaded organic phase is regulated to be (0.20-0.35):1.0, and the volume ratio of the aqueous phase to the organic phase is (0.1-3.0):1.
0.
2. The method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater according to claim 1, characterized in that: During the precipitation stripping process, stripping and precipitation of tantalum / niobium are carried out simultaneously, and the molar ratio of boron in the boron-containing liquid and fluorine in the tantalum-niobium loaded organic phase is regulated to be (0.25-0.29):1.0, and the volume ratio of the aqueous phase to the organic phase is (0.25-2):1.
0.
3. A method for precipitation stripping of tantalum-niobium loaded organic phase and treatment of stripping wastewater according to claims 1 and 2, characterized in that: The boron-containing liquid uses at least one of metaborate, metaboric acid and boric acid as solute.
4. The method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater according to claim 1, characterized in that: The three-phase separation is to separate tantalate or niobic acid precipitate, blank organic phase and fluorine-boron-containing wastewater from the mixed phase formed by back extraction precipitation by means of standing, liquid separation, centrifugation, sedimentation, filtration and the like.
5. The method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater according to claim 1, characterized in that: The tantalum-niobium loaded organic phase is an extraction phase of tantalum or niobium in a hydrofluoric acid solution, and the tantalum or niobium exists in the form of fluorine complex ions.
6. The method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater according to claim 1, characterized in that: The blank organic phase contains at least one of methyl isobutyl ketone, sec-octanol, tributyl phosphate, cyclohexanone and acetamide.
7. The method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater according to claim 1, characterized in that: The crystallization treatment is to prepare fluoroborate by evaporating and crystallizing the fluorine-boron-containing wastewater or adding potassium salt for precipitation.
8. The method for precipitation stripping of organic phase loaded with tantalum and niobium and treatment of stripping wastewater according to claim 1, characterized in that: The washing is performed by using pure water or boron-containing liquid; the calcination is performed at a high temperature of 600-1000°C in an atmosphere containing oxygen or water vapor.