High-strength rare earth aluminosilicate glass and preparation method thereof
By adding rare earth elements to high-aluminum glass, the network structure tightness of the glass is improved, the production difficulty and cost problems brought about by high alumina are solved, high-performance cover glass is realized, and rare earth resources are effectively utilized, which meets the The market demand for high strength and hardness.
Patent Information
- Application Number
- CN202411115018.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
After increasing the alumina content, the production difficulty of existing high-alumina glass increases, which is costly and difficult to meet the performance requirements of high strength, high hardness, compression resistance and scratch resistance. At the same time, the problem of rare earth element backlog has not been solved.
On the basis of maintaining high alumina content, rare earth elements, such as lanthanum cerium, are added as the main component of glass, to improve the network structure tightness of glass through rare earth oxides, reduce production difficulty and cost, and replace part of aluminum with rare earth elements and Lithium element optimizes the chemical strengthening process of glass.
It has achieved improvements in high strength, high hardness, compression resistance, scratch resistance and impact resistance, reduced the production cost of high-aluminum glass, solved the problem of rare earth element backlog, and expanded the application field of rare earth elements in glass.
Smart Images

Figure CN118993530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass, and in particular relates to a high-strength rare earth aluminosilicate glass and a preparation method thereof. Background Art
[0002] With the continuous progress of smart displays, especially smart phones, electronic glass has developed by leaps and bounds. As glass has the advantages of exquisite appearance, mature technology, excellent performance and low cost, electronic glass as the cover glass of smart phones has gradually replaced the original metal shell. At present, the application of smart phone cover glass has become an important part of the application of electronic glass. Cover glass, also known as window protective glass or touch screen protective glass, is a transparent lens added to the outside of the display screen to protect the touch module and display module. According to the chemical composition, cover glass is mainly divided into soda-lime silicate glass, soda-aluminum silicate glass, and lithium-aluminum silicate glass (sodium aluminum and lithium aluminum are both alkali-aluminum silicate glass).
[0003] Ordinary soda-lime glass can no longer meet the required performance, and it is difficult to improve its performance even after chemical strengthening. As a protective cover glass, when in contact with the outside world, it needs to meet the requirements of thickness and transparency, as well as high strength, high hardness, compression resistance, scratch resistance and impact resistance. Currently, the most widely used is high-aluminum glass, which is stronger than ordinary soda-lime glass and has stronger ion exchange capacity.
[0004] High-aluminum glass is already the preferred glass cover for touch screens of electronic products, and the aluminum oxide content in the high-aluminum glass components in the current market has been on a high and rising trend. The increase in aluminum oxide content can effectively improve the scratch resistance of the glass, and also continuously increase the height of the mobile phone's drop. Patent document CN116903248A provides a composition for preparing high-aluminum glass, wherein the aluminum oxide content reaches 14-23wt%, has excellent mechanical properties and reaches a surface compressive stress value of more than 980MPa after ion exchange, but the Young's modulus of its high-aluminum glass is ≤75GPa, and the stress layer depth after ion exchange is 30-42μm. It is far lower than the performance requirements of the glass in the present invention and cannot meet market demand. Patent document CN113149428A discloses a method for preparing high-aluminum glass and high-aluminum tempered glass, so that the aluminum oxide content of the glass reaches 25-31wt%, has high strength and surface hardness, and the Vickers hardness after ion strengthening reaches 680Kgf / mm 2As mentioned above, high content of aluminum oxide can make the chemical stability of the glass body better, and the tempered glass after ion exchange has a higher surface compressive stress value (500-1000MPa) and a deeper compressive stress layer depth (≥100μm). However, due to the introduction of too much aluminum oxide, the viscosity of the glass liquid is high, the surface tension is large, and the melting, clarification, and homogenization are more difficult. In the production process, it is easy to have many bubbles, glass tendons, lines, stripes and other defects. It is difficult to use general production technology (float process) for production, which greatly increases the cost of aluminosilicate glass. In patent document CN111995243A, 0-15mol% of lithium oxide and 6-20mol% of sodium oxide are added, and in patent document CN112010552 A, 9.5-20wt% of sodium oxide and 3-8wt% of lithium oxide are added to make up for the production difficulty caused by high content of aluminum oxide, and also create good conditions for secondary ion exchange. The depth of its ion exchange layer can reach more than 100μm and obtain a surface compressive stress of more than 800MPa, making it more impact-resistant. However, due to the rapid development of lithium batteries, the price of lithium has remained high, which is much more expensive than other materials. This directly leads to the production cost of cover glass becoming very high. Reducing the amount of lithium oxide to reduce production costs while ensuring ion exchange, and reducing the melting temperature and viscosity to reduce the process difficulty on the basis of high-content aluminum oxide are the problems that need to be solved at present. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a high-strength rare earth aluminosilicate glass and a preparation method thereof. The present invention adds a certain amount of rare earth elements on the basis of maintaining a high alumina content, and uses rare earth elements as one of the main components of the glass. Compared with alkali metal and alkaline earth metal oxides, rare earth oxides have higher ion field strength and dissociation energy, which will make the network structure of the glass more compact, and can greatly improve the performance of the glass in terms of wear resistance, optical properties and chemical stability. With the continuous mining and separation of rare earths, light rare earths separated from praseodymium and neodymium, especially lanthanum and cerium, have been backlogged. Using rare earth elements in glass production can not only significantly reduce costs, but also effectively solve the problem of rare earth backlog. At the same time, rare earth elements will also replace part of aluminum and lithium elements, and can further reduce the production difficulty and cost of high aluminum glass without affecting the subsequent chemical strengthening of glass, and can also meet the high strength, high hardness, compression resistance, scratch resistance and impact resistance required by the performance of cover glass on the market. And the strengthened high aluminum glass can achieve a higher compressive stress and surface compression layer depth.
[0006] The present invention is achieved through the following technical solutions.
[0007] In a first aspect, the present invention provides a high-strength rare earth aluminosilicate glass, which is made of a batch of raw materials including the following parts by weight: 48-58 parts SiO 2 , 15-24 parts Al 2 O 3 、9-21 RE 2 O 3 , 1-4 parts MgO, 5-10 parts Na 2 O, 1-6 parts Li 2 O, 0.5-1.5 parts K 2 O.
[0008] In some embodiments, the batch material further includes 0.2-0.5 parts of Sb 2 O 3 .
[0009] In some embodiments, the RE 2 O 3 Including La 2 O 3 、CeO 2 and Y 2 O 3 Preferably, (La 2 O 3 +CeO 2 +Y 2 O 3 ) accounts for ≥9% of the total composition, (La 2 O 3 +CeO 2 +Y 2 O 3 ) is designed to have a content of ≥9%, which can improve the hardness, Young's modulus and fracture toughness of the glass; further preferably, CeO 2 / La 2 O 3 The mass ratio of Y is 0.0-0.8, and 2 O 3 / La 2 O 3 The mass ratio of is 0.0-1.0. By controlling the content ratio of the above components, the hardness, Young's modulus and fracture toughness of the glass can be further improved.
[0010] In some embodiments, MgO / Al 2 O 3 The mass ratio of MgO / Al is 0.04-0.3. 2 O 3 Designing the mass ratio within the above range can reduce the glass melting temperature and improve the glass stability.
[0011] In some embodiments, RE2 O 3 / Al 2 O 3 The mass ratio of RE is 0.3-1.4. 2 O 3 / (Al 2 O 3 +Li 2 O) is 0.3-1.35. Controlling the above component content relationship can effectively reduce the glass melting temperature and high temperature viscosity.
[0012] In some embodiments, (Na 2 O+Li 2 O+K 2 O) accounts for ≤20% of the total composition, which can further improve the ion exchange depth.
[0013] SiO 2 As a network former, it is an essential component of glass. Silicon-oxygen tetrahedron [SiO 4 ] as the basic structural unit to form the main glass network structure, improve the chemical stability, mechanical properties and thermal stability of the glass, and reduce its crystallization tendency. 2 The content of SiO2 will increase the melting temperature of the glass, increase the difficulty of melting and production cost, and also cause defects such as a large number of small bubbles in the glass. 2 The quality accounts for 48-58%.
[0014] Al 2 O 3 As a network intermediate, it is a minor structural component of the glass skeleton. 2 O 3 It is one of the necessary components and belongs to the network intermediate composition. In the high alkali content glass component, the alkali ion is 3+ The ions balance the charge, making most of the aluminum oxide tend to become aluminum-oxygen tetrahedrons, forming the main network structure of the glass, thereby improving the stability and mechanical properties of the glass. 2 O 3 The volume of the aluminum-oxygen tetrahedron formed in the glass is larger than that of the silicon-oxygen tetrahedron, which will cause the glass volume to expand, thereby reducing the density of the glass, providing an exchange channel for the glass in the ion exchange process, and increasing the depth of the glass compressive stress layer. 2 O 3 The Al2O3 glass has a high strain point temperature, so that the glass can maintain a high compressive layer stress after ion exchange. 2 O 3 The mass percentage is at least ≥15%. 2 O3 It is an extremely refractory oxide. It can quickly increase the high-temperature viscosity of glass, making it more difficult to clarify and homogenize the glass, and greatly increase the concentration of bubble defects in the glass. Therefore, Al in glass 2 O 3 The quality of the products does not exceed 24%.
[0015] La 2 O 3 As a rare earth oxide, it can form La-O-Si and La-O-Al bonds with silicon-oxygen tetrahedrons and aluminum-oxygen hexahedrons in glass to form more stable structural units, thereby increasing its structural stability and glass density. 2 O 3 The addition of can reduce the glass viscosity and melting temperature, promote the melting and preparation process of glass, and play the role of flux. As a glass network modifier, it can significantly improve the mechanical strength and stiffness of aluminosilicate glass, and can greatly improve the glass performance in terms of wear resistance, optical properties and chemical stability. 2 O 3 The dissociation energies of La-O and YO bonds are 799 and 715 kJ / mol, respectively, which are very close to the dissociation energy of Si-O bonds (798 kJ / mol) and will not lead to a significant decrease in the intrinsic strength of the glass. 3+ Rare earth ions with high ionic field strength are filled into the glass network as network modifiers, which can also improve the physical and chemical properties of the glass. 2 It can also improve the mechanical and optical properties of glass. 2 O 3 +CeO 2 +Y 2 O 3 The mass proportion of Rare Earth Oxide is at least greater than 9%. Rare earth oxide is one of the main components of glass. If the content exceeds a certain level, it will exceed the glass formation region and cause serious devitrification. Therefore, the present invention limits La 2 O 3 +CeO 2 +Y 2 O 3 The quality of the products does not exceed 21%.
[0016] MgO is an alkaline earth metal oxide, which is an external component of the glass network. It destroys the glass network structure, reduces the melting temperature of the glass, plays a role in fluxing, and can also improve the stability of the glass. It is beneficial to clarify and prevent glass crystallization. However, if it is higher than a certain content, it may hinder the ion exchange rate during the chemical strengthening process. Therefore, in the present invention, the mass proportion of MgO is limited to 1-4%.
[0017] Na2 O is one of the necessary components for ion exchange. When the glass contains sufficient Na 2 O can provide a large amount of Na + Can be combined with K in molten salt + Ion exchange occurs, resulting in high compressive stress on the glass surface. 2 O can provide a large amount of free oxygen, thereby destroying the Si-O bond of the silicon-oxygen network structure and reducing the viscosity and melting temperature of the glass. 2 The mass percentage of O should be no less than 5%. 2 When the content of O is too high, the thermal expansion coefficient of the glass will increase and the chemical stability and mechanical properties of the glass will decrease. 2 The mass percentage of O is not more than 10wt%.
[0018] Li 2 O is one of the main components for ion exchange. Due to its polarization characteristics, it can effectively reduce the viscosity of glass and lower the melting temperature of glass, making it an excellent flux. + The ion radius of NaNO is very small, so it can fill the gaps inside the vitreous body and balance the free oxygen. 3 With KNO 3 In the mixed molten salt, Li in the glass + With Na in molten salt + Ion exchange can quickly obtain a high compressive stress layer depth, so that the glass has good compression and impact resistance. 2 The mass proportion of O is not less than 1wt%. If Li 2 The concentration of O is not enough, and Li + with Na + The exchange amount will be insufficient, and it will be difficult to obtain the required stress layer depth. 2 If the mass ratio of O is too high, the production cost of glass will be greatly increased. At the same time, the thermal expansion coefficient of glass will also increase with the increase of Li 2 O increases significantly, which is not conducive to the stability and durability of the glass. 2 The mass proportion of O is no more than 6%.
[0019] K 2 O、Na 2 O and Li 2 O is an alkali metal oxide, which can increase the ion exchange rate and deepen the compressive stress layer, and can also play a role in breaking the network, reducing the viscosity and melting temperature of the glass. 2 O and Na 2 The simultaneous presence of K and O can form a mixed alkali effect, which can optimize a series of glass properties. +The radius is smaller than Na + and Li + The maximum field strength is small, so the ability to combine with oxygen is weak. 2 O will hinder Li + and Na + The ion exchange will reduce the surface stress value. 2 The mass proportion of O is preferably 0.5-1.5 wt%.
[0020] In a second aspect, the present invention provides a method for preparing high-strength rare earth aluminosilicate glass, comprising the following steps:
[0021] (1) mixing the batch materials for preparing high-strength rare earth aluminosilicate glass uniformly, maintaining the temperature at 1500-1630° C. for 3-5 hours, and melting the mixture to obtain glass liquid;
[0022] (2) forming the molten glass liquid, and then annealing it at a temperature of 600-700°C for 2-5 hours; and
[0023] (3) The temperature is lowered to a temperature near the strain point at a rate of less than 1°C / min, and then naturally cooled to room temperature to obtain the base glass.
[0024] In some embodiments, after the base glass is immersed in a 5% HCl solution at 95° C. for 24 hours, the weight loss of the base glass is no more than 4 mg / cm 2 .
[0025] In some embodiments, after the base glass is immersed in a 5% NaOH solution at 95° C. for 6 hours, the weight loss of the base glass is no more than 2.5 mg / cm 2 .
[0026] In some embodiments, the base glass has a light transmittance greater than 90% in the visible light band.
[0027] In some embodiments, the Young's modulus of the base glass is ≥80 GPa, preferably ≥90 GPa.
[0028] In some embodiments, the Vickers hardness of the base glass is ≥ 630 Kgf / mm 2 , preferably ≥660Kgf / mm 2 .
[0029] In some embodiments, the fracture toughness of the base glass is ≥1.40 MPa·m 1 / 2 , preferably ≥1.5MPa·m 1 / 2 .
[0030] In some embodiments, the preparation method further comprises chemically strengthening the base glass, and the chemical strengthening operation comprises the following steps:
[0031] (4) First ion exchange: The base glass is placed in a first molten salt for first ion exchange, wherein the first molten salt comprises KNO 3 and NaNO 3 , the first molten salt NaNO 3 / KNO 3 The mass ratio is 2.0-4.0:1; the temperature of the first ion exchange is 350-450°C and the time is 3-8h; and
[0032] (5) Secondary ion exchange: The glass after the first ion exchange is placed in a second molten salt for secondary ion exchange. The second molten salt is 100 wt% KNO 3 The secondary ion exchange temperature is 400-550°C and the time is 1-3h; and reinforced glass is obtained.
[0033] In some embodiments, the strengthened glass has a surface compressive stress value of ≥800 MPa, preferably ≥900 MPa, and more preferably ≥1000 MPa, and a compressive stress layer depth of 80 μm or more.
[0034] In some embodiments, the Vickers hardness of the strengthened glass is higher than 680 kgf / mm 2 , preferably higher than 700kgf / mm 2 , fracture toughness ≥1.4MPa·m 1 / 2 , preferably ≥1.6MPa·m 1 / 2 .
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The present invention introduces rare earth oxide RE 2 O 3 , making it the second most abundant aluminosilicate glass after SiO 2 and Al 2 O 3 One of the main components of rare earth aluminosilicate glass, rare earth elements La, Y, Ce replace part of the original Li element in the glass. Without affecting the subsequent ion exchange, it can solve the problem of excessively high glass production costs due to excessive lithium oxide content in the above patent, and can greatly reduce the raw material cost of high aluminum glass. At the same time, it can solve the backlog problem caused by the separation of rare earth elements.
[0037] 2. The rare earth aluminosilicate glass of the present invention can promote the melting and preparation process of glass by introducing rare earth oxides, and the addition of rare earth elements La, Y, and Ce, and plays the role of flux, which can solve the problems of high viscosity of glass liquid, high surface tension, high glass melting temperature, etc. caused by excessively high alumina content in the above patents. It can reduce the technical requirements for melting glass, greatly reduce high-temperature energy consumption, and also reduce the loss of molds and equipment.
[0038] 3. On the basis of overcoming the deficiencies of the above-mentioned prior art, the present invention can expand the application field of rare earth elements lanthanum, cerium and yttrium on glass. Rare earth oxides have greater ion field strength and higher dissociation energy than alkali metal and alkaline earth metal oxides. The addition of La, Ce and Y elements makes the glass have better mechanical strength and rigidity, and improves wear resistance, optical properties and chemical stability. Its Young's modulus, shear modulus and Vickers hardness are significantly greater than those of the traditional cover glass sodium calcium silicon system and the popular alkali aluminosilicate glass system, and the rare earth aluminosilicate glass also exhibits good thermal stability. Through the overall implementation of the technology, not only the performance meets the requirements of high hardness, high elasticity and high fracture toughness of the cover glass for touch screen protection, but more importantly, it can achieve high content and high value application of high-abundance rare earth elements in the cover glass for touch screen protection, and promote the balanced utilization of rare earth resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a Vickers indentation morphology image of the basic glass before ionomer strengthening at a load of 1.96N in Example 1 of the present invention;
[0040] Figure 2 This is a Vickers indentation morphology image of the basic glass after ionomer strengthening at a load of 1.96N in Example 1 of the present invention;
[0041] Figure 3 1 is the transmittance curve of the glass in Examples 1-4 of the present invention. DETAILED DESCRIPTION
[0042] The present invention is described in detail below in conjunction with specific comparative examples, embodiments and drawings. This embodiment and some comparative examples are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0043] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.
[0044] Example:
[0045] 1. Preparation of rare earth aluminosilicate based glass
[0046] Examples 1-6 of the present invention and comparative examples 1-2, 5-6 are prepared by the following method: the basic glass raw materials (batch materials) are mixed uniformly according to the proportions in Table 1, and then the mixture is transferred to a platinum crucible, and the platinum crucible is placed in a silicon-molybdenum rod high-temperature furnace, and the temperature is gradually increased to 1500-1630°C (for example, 1550°C), and the temperature is kept for 3-5 hours (for example, 4 hours), and the bubbles are accelerated to be discharged and the glass is homogenized by stirring. After melting, the melt (i.e., glass liquid) is formed, and then annealed at an annealing temperature of 600-700°C (for example, 650°C) for 2-5 hours (for example, 3.5 hours), and then the temperature is reduced to a temperature near the strain point at a rate of less than 1°C / min, and then naturally cooled to room temperature to obtain the basic glass. Comparative Example 3 is prepared according to Example 1 in patent document CN112010552A, and Comparative Example 4 is prepared according to Example 3 in patent document CN116903248A.
[0047] 2. Preparation of rare earth aluminosilicate chemically strengthened glass:
[0048] The base glasses (thickness 0.7 mm) prepared in Examples 1-6 and Comparative Examples 1-2 and 5-6 were placed in a first molten salt (NaNO 3 / KNO 3 The first ion exchange was carried out at a temperature of 450°C for 4 h, and then the second molten salt (100 wt% KN0 3 ) for secondary ion exchange, the ion exchange temperature is 420°C, and the time is 2h. Table 2 shows the performance test results of the basic glass before and after ion exchange in the corresponding embodiments and comparative examples of Table 1, including acid and alkali resistance, Young's modulus, Vickers hardness, fracture toughness, surface compressive stress and stress layer depth.
[0049] Description of the test method in Table 2:
[0050] 1. 5% HCl weight loss (mg / cm 2 ): The cleaned and dried glass sample was immersed in a 5% HCl solution, the temperature was set to 95°C, and the immersion time was 24 hours; a 1 / 10,000 precision balance was used to measure the change in glass mass before and after immersion, and the weight loss ratio of the glass in the 5% HCl solution was calculated by measuring the surface area of the glass.
[0051] 2. 5% NaOH weight loss (mg / cm 2): The cleaned and dried glass sample was immersed in a 5% NaOH solution, the temperature was set to 95°C, and the immersion time was 6 hours; a 1 / 10,000 precision balance was used to measure the change in glass mass before and after immersion, and the weight loss ratio of the glass in the 5% NaOH solution was calculated by measuring the glass surface area.
[0052] Table 1: Glass compositions of Examples 1-6 and Comparative Examples 1-6
[0053]
[0054] Table 2: Performance test of the glasses of Examples 1-6 and Comparative Examples 1-6 before and after ion exchange
[0055]
[0056] Figure 1 and Figure 2 The 1.96N load Vickers indentation morphology of the rare earth aluminosilicate glass of Example 1 of the present invention before and after ion exchange. The Vickers hardness of the glass of Example 1 before ion exchange is 663Kgf / mm 2 , the Vickers hardness after ion exchange is 702Kgf / mm 2 . This shows that ion exchange improves the mechanical properties of glass.
[0057] Figure 3 1 is the transmittance curve of the glass of Examples 1 to 4. The transmittance of the rare earth aluminosilicate glass of the present invention in the visible light band (380nm-780nm) reaches more than 90%.
[0058] From the results in Table 2, it can be seen that the Young's modulus of the base glasses of Examples 1-6 all exceeded 90 GPa, and the weight loss after immersion in a 5% HCl solution at 95°C for 24 hours was 3.2-3.9 mg / cm 2 After immersion in 5% NaOH solution at 95°C for 6 hours, the weight loss of the glass was 1.9-2.3 mg / cm 2 . It has excellent mechanical properties and chemical stability. After ion exchange, the Vickers hardness and fracture toughness of the rare earth aluminosilicate glass of Examples 1-6 are improved. The Vickers hardness of Examples 1-6 after improvement reaches 700Kgf / mm 2 Above, fracture toughness reaches 1.62-1.82MPa·m 1 / 2 The glass of Examples 1-6 can achieve a surface compressive stress CS ≥ 1000 MPa and a stress layer depth DOL > 80 μm, which is beneficial for improving the drop resistance and can better meet the application requirements of touch screen protection glass.
[0059] The Young's modulus, Vickers hardness, fracture toughness and chemical stability of the glasses in Comparative Examples 1 and 2 are much lower than those in Examples 1-6. As can be seen from the glass composition table in Table 1, the rare earth oxide La in the glass components of Comparative Examples 1 and 2 is 2 O 3 +CeO 2 +Y 2 O 3 The content is far less than 9wt%. Without sufficient rare earth elements La, Ce, and Y, the elastic modulus is less than 70GPa, and the Vickers hardness does not exceed 640Kgf / mm after ion strengthening. 2 At the same time, the surface compressive stress (<800Mpa) and stress layer depth (<60μm) of the glass did not meet the corresponding performance requirements, and the glass's drop resistance was poor.
[0060] Comparative Example 3 is Example 1 in patent document CN112010552A. It can be seen from the glass components in Table 1 that the lithium oxide content in the glass components of Comparative Example 3 is 7.45wt% and the sodium oxide content is 11.82wt%, which are much higher than the glasses of Examples 1-6, and exceed the component content range of lithium oxide and sodium oxide in the present invention. From the results in Table 2, it can be seen that its Young's modulus is 76GPa, which is much lower than the glasses of Examples 1-6. Due to the high content of lithium oxide and sodium oxide in the components, the stress layer depth DOL after ion exchange reaches 117μm. But the Vickers hardness is only 642Kgf / mm 2 The high content of lithium oxide in the glass component of Comparative Example 3 greatly increases the production cost, and the performance is lower than that of the glasses of Examples 1-6 in the present invention except for the depth of the stress layer.
[0061] Comparative Example 4 is Example 3 in patent document CN116903248A. It can be seen from the glass components in Table 1 that the aluminum oxide content in the glass components of Comparative Example 4 is 23wt%, the sodium oxide content is 22wt%, and the lithium oxide content is 0.3wt%. The fluxing effect is obtained by adding a high content of sodium oxide. From the results in Table 2, it can be seen that the Young's modulus of the glass in Comparative Example 4 is 73GPa, which is lower than that of the glass in Examples 1-6. Due to the extremely high sodium oxide content, the surface compressive stress after ion exchange can reach 1150Mpa, but the extremely low lithium oxide content makes its stress layer depth only 42μm. Although the glass component of Comparative Example 4 solves the cost problem caused by lithium oxide and the high-temperature melting problem of high-aluminum glass, its mechanical properties are lower than those of Examples 1-6 in the present invention, and the Vickers hardness after ion exchange is only 638Kgf / mm 2 , and the lower stress layer depth makes the drop resistance poorer.
[0062] The rare earth oxide La in the glass component of Comparative Example 5 2 O 3+CeO 2 +Y 2 O 3 The content of La exceeds 21wt%, and its component is no longer in the corresponding glass formation region in the phase diagram. It is found that the glass of Comparative Example 5 has a large area of white devitrification area, which cannot meet the requirements of touch screen protection glass transparency. 2 O 3 +CeO 2 +Y 2 O 3 The content is less than 9wt%, and CeO 2 The content of is too high, making the glass appear brown-black. Due to the lower rare earth content, the Young's modulus, Vickers hardness, fracture toughness and chemical stability of the glass are much lower than those of the glass of Examples 1-6.
[0063] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-strength rare earth aluminosilicate glass, characterized in that: The high-strength rare earth aluminosilicate glass is made of a batch of raw materials including the following parts by weight: 48-58 parts of SiO2, 15-24 parts of Al2O3, 9-21 parts of RE2O3, 1-4 parts of MgO, 5-10 parts of Na2O, 1-6 parts of Li2O, and 0.5-1.5 parts of K2O.
2. The high-strength rare earth aluminosilicate glass according to claim 1, characterized in that: The batch material also includes 0.2-0.5 parts of Sb2O3.
3. The high-strength rare earth aluminosilicate glass according to claim 1 or 2, characterized in that: The RE2O3 includes La2O3, CeO2 and Y2O3; preferably, the mass ratio of (La2O3+CeO2+Y2O3) to the total components is ≥9%; further preferably, the mass ratio of CeO2 / La2O3 is 0.0-0.8, and the mass ratio of Y2O3 / La2O3 is 0.0-1.
0.
4. The high-strength rare earth aluminosilicate glass according to any one of claims 1 to 3, characterized in that: The mass ratio of MgO / Al2O3 is 0.04-0.3; and / or The mass ratio of RE2O3 / Al2O3 is 0.3-1.4; and / or The mass ratio of RE2O3 / (Al2O3+Li2O) is 0.3-1.
35.
5. The high-strength rare earth aluminosilicate glass according to any one of claims 1 to 4, characterized in that: The mass ratio of (Na2O+Li2O+K2O) to the total components is ≤20%.
6. The method for preparing the high-strength rare earth aluminosilicate glass according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) mixing the batch materials for preparing high-strength rare earth aluminosilicate glass uniformly, maintaining the temperature at 1500-1630° C. for 3-5 hours, and melting the mixture to obtain glass liquid; (2) forming the molten glass liquid, and then annealing it at a temperature of 600-700°C for 2-5 hours; and (3) The temperature is lowered to a temperature near the strain point at a rate of less than 1°C / min, and then naturally cooled to room temperature to obtain the base glass.
7. The preparation method according to claim 6, characterized in that: After the base glass is immersed in a 5% HCl solution at 95° C. for 24 hours, the weight loss of the base glass is no more than 4 mg / cm 2 ; and / or After the base glass is immersed in a 5% NaOH solution at 95° C. for 6 hours, the weight loss of the base glass is no more than 2.5 mg / cm 2 ; and / or The light transmittance of the base glass in the visible light band is greater than 90%; and / or The Young's modulus of the base glass is ≥80 GPa, preferably ≥90 GPa; and / or The Vickers hardness of the base glass is ≥630Kgf / mm 2 , preferably ≥660Kgf / mm 2 ; and / or The fracture toughness of the base glass is ≥1.40 MPa·m 1 / 2 , preferably ≥1.5MPa·m 1 / 2 .
8. The preparation method according to claim 6 or 7, characterized in that: The preparation method further comprises chemically strengthening the base glass, wherein the chemical strengthening operation comprises the following steps: (4) first ion exchange: placing the base glass into a first molten salt for first ion exchange, wherein the first molten salt comprises KNO3 and NaNO3, and the mass ratio of NaNO3 / KNO3 in the first molten salt is 2.0-4.0:1; the temperature of the first ion exchange is 350-450°C, and the time is 3-8h; and (5) Secondary ion exchange: The glass after the first ion exchange is placed in a second molten salt for secondary ion exchange, wherein the second molten salt is 100wt% KNO3; the temperature of the secondary ion exchange is 400-550°C and the time is 1-3h; and strengthened glass is obtained.
9. The preparation method according to claim 8, characterized in that: The tempered glass has a surface compressive stress value of ≥800 MPa, preferably ≥900 MPa, and more preferably ≥1000 MPa, and a compressive stress layer depth of 80 μm or more.
10. The preparation method according to claim 8 or 9, characterized in that: The Vickers hardness of the tempered glass is higher than 680 kgf / mm 2 , preferably higher than 700kgf / mm 2 , fracture toughness ≥1.4MPa·m 1 / 2 , preferably ≥1.6MPa·m 1 / 2 .
Citation Information
Patent Citations
Glass for chemical strengthening, chemically strengthened glass and method for manufacturing chemically strengthened glass
CN109843823A
Low-viscosity and high-aluminum glass, preparation method and applications thereof
CN111018346A
High-modulus glass fiber composition and glass fiber and composite material thereof
CN111747654A
Glass, chemically tempered glass, and method for producing same
CN113905992A
Chemically strengthened glass article and method for producing same
CN114929641A
Cited By
High-strength photoelectric glass and preparation method thereof
CN120483521A