Brown medium-boron medicinal glass and preparation method thereof
By preparing brown traditional boron medicinal glass with specific ratios, the shortcomings of existing glasses in acid and alkali resistance and light-shielding properties are solved, and the high-performance needs of medicinal packaging materials are achieved, ensuring the stability and safety of drugs.
Patent Information
- Application Number
- CN202411008928.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing soda calcium and low borosilicate glasses cannot meet the high requirements of new drugs for acid and alkali resistance and light shading in medicinal packaging materials, resulting in the threat of drug stability and safety.
Develop a brown traditional boron medicinal glass through specific raw material ratios and preparation methods, including quartz sand, alumina, sodium carbonate, feldspar, borax, potassium carbonate, barium carbonate, sodium sulfate, carbon powder and brown crushed glass , forming glass with excellent acid resistance, alkali resistance and good light shielding effect.
The glass has been improved with acid resistance, alkali resistance and light shielding, ensuring the stability and safety of drugs, and meeting the high performance needs of medicinal packaging materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of glass preparation, and in particular to a brown medium-boron medicinal glass and a preparation method thereof. Background Art
[0002] With the country's adjustment of the pharmaceutical packaging material industry structure, the production of Class I water-resistant pharmaceutical glass products is encouraged, and the use of low-borosilicate glass and soda-lime glass is not recommended. It is required that the quality and performance of packaging materials and containers used for injections must not be lower than that of reference preparations to ensure that the quality of the drugs is consistent with the reference preparations.
[0003] Glass pharmaceutical packaging materials have good chemical stability, can be directly in contact with drugs, are easy to clean, and will not deform or leak after high-temperature disinfection and sterilization. However, as it is widely used in the field of medical packaging glass, many new drugs have higher requirements for its acid and alkali resistance. At the same time, some special drugs become ineffective due to light exposure. The acid and alkali resistance or light-shielding properties of today's soda-lime and low-borosilicate glass can no longer meet our needs at the same time. It is urgent to improve the performance of glass pharmaceutical packaging materials to ensure the stability and safety of drugs. Summary of the invention
[0004] The purpose of the present application is to overcome the defects existing in the prior art and to provide a brown medium-boron medicinal glass and a preparation method thereof. The brown medium-boron medicinal glass prepared in the present application has excellent acid and alkali resistance, relatively stable coloring, and good shading effect.
[0005] The first aspect of the present application provides a brown medium-boron medicinal glass. Based on the total weight of the raw materials for preparing the medium-boron medicinal glass, the components of the brown medium-boron medicinal glass include, by mass percentage, 35.0%-37.0% quartz sand, 2.0%-5.0% alumina, 1.0%-3.0% sodium carbonate, 6.0%-2.0% feldspar, 12.0%-14.0% borax, 1.0%-3.0% potassium carbonate, 3.0%-1.0% barium carbonate, 1.0%-3.0% calcium carbonate, 0.4%-0.1% sodium sulfate, 0.1%-0.6% carbon powder, and 35.0% brown broken glass.
[0006] In some embodiments, based on the total weight of the medium-boron pharmaceutical glass raw material, the mass percentage of sodium carbonate + potassium carbonate is 3-5%, and / or the mass percentage of barium carbonate + calcium carbonate is 3-5%, and / or the mass percentage of sodium sulfate and carbon powder is 0.7-0.8%.
[0007] In some embodiments, based on the total weight of the raw materials for preparing medium-boron medicinal glass, the components of the brown medium-boron medicinal glass include, by mass percentage: 36.0% quartz sand, 3.5% aluminum oxide, 2.0% sodium carbonate, 4.5% feldspar, 13.0% borax, 2.0% potassium carbonate, 2.0% barium carbonate, 2.0% calcium carbonate, 0.3% sodium sulfate, 0.5% carbon powder, and 35% brown broken glass.
[0008] In some embodiments, based on the total weight of the medium-boron pharmaceutical glass raw material, the mass percentage of sodium carbonate + potassium carbonate is 4%, and / or the mass percentage of barium carbonate + calcium carbonate is 4%, and / or the mass percentage of sodium sulfate and carbon powder is 0.8%.
[0009] In some embodiments, the content of silicon dioxide in the quartz sand is greater than 98.5%.
[0010] The second aspect of the present application provides a method for preparing brown medium-boron medicinal glass, which is used for the aforementioned brown medium-boron medicinal glass, comprising the steps of:
[0011] Evenly mix quartz sand, alumina, sodium carbonate, feldspar, borax, potassium carbonate, barium carbonate, calcium carbonate, sodium sulfate, carbon powder and brown broken glass;
[0012] The mixed material is heated to a uniform molten state to obtain a high-quality brown medium-boron medicinal glass liquid;
[0013] The brown medium-boron medicinal glass liquid is drawn into a glass tube of a certain specification;
[0014] The glass tube is roughly cut after it cools down naturally, and then both ends of the glass tube are cut as a whole, and then the final round mouth is made on the end of the glass tube.
[0015] In some embodiments, the mixing uniformity is greater than 95%.
[0016] In some embodiments, the mixture is heated to a temperature of 1550°C-1600°C.
[0017] In some embodiments, the cooling temperature of the glass tube is 180-220°C.
[0018] In some embodiments, the device for heating and melting the mixed material is a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a mixed heating furnace combining a flame furnace and an all-electric furnace.
[0019] The medium-boron medicinal glass prepared in this application has excellent acid and alkali resistance, and the coloring is relatively stable, and the shading effect is good. SiO2, Al2O3 and B2O3 in the glass work together through mechanisms such as enhancing the network structure, balancing the charge, improving the compactness and stability, and jointly improve the acid resistance of the glass. At the same time, by adding other oxides, such as alkali metal oxides, the compactness of the glass is increased, a protective layer or barrier layer is formed, and the direct contact between SiO2 and the alkaline ions is reduced, which further improves the alkali resistance of the medium-boron medicinal glass. The coloring of the brown medium-boron silicon glass tube requires the dual effects of the colorant sodium sulfate and the reducing agent carbon powder. The addition of sodium sulfate will change the molecular structure of the glass, produce new absorption bands, thereby affecting the propagation and reflection of light in the glass, and achieving the coloring effect. In the glass production process, carbon powder can accelerate the decomposition process of sodium sulfate as a reducing agent. Sodium sulfate decomposes at high temperature to produce gases such as hydrogen sulfide, which react with the oxides in the glass to help clarify and color the glass. Therefore, the medium-boron medicinal glass provided in this application has good acid and alkali resistance and good shading effect. DETAILED DESCRIPTION
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the description and claims of this application and any variations thereof are intended to cover non-exclusive inclusions.
[0021] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0022] In order to solve the problems raised in the background technology, the first aspect of the present application provides a brown medium-boron medicinal glass. Based on the total weight of the raw materials for preparing the medium-boron medicinal glass, the components of the brown medium-boron medicinal glass include, by mass percentage: 35.0%-37.0% quartz sand, 2.0%-5.0% alumina, 1.0%-3.0% sodium carbonate, 6.0%-2.0% feldspar, 12.0%-14.0% borax, 1.0%-3.0% potassium carbonate, 3.0%-1.0%, 1.0%-3.0% calcium carbonate, 0.4%-0.1% sodium sulfate, 0.1%-0.6% carbon powder, and 35.0% brown broken glass.
[0023] The components of the brown medium-boron pharmaceutical glass in the present application include silicon dioxide, aluminum oxide, boron oxide and other components, wherein silicon dioxide constitutes the skeleton of the glass and is the guarantee of the chemical stability and durability of the glass, and components such as boron oxide and aluminum oxide improve the mechanical properties of the glass and the chemical stability of the glass to a certain extent. At the same time, during the production and preparation process, aluminum oxide can have a strong coupling reaction with the alkali ions in the glass, effectively inhibiting the migration of alkali ions, improving the acid resistance and alkali resistance of the glass, reducing the tendency of the glass to peel off, and improving the chemical stability of the glass; however, as the aluminum oxide content increases, the viscosity of the glass will increase, causing difficulties in molding, and defects such as stripes and nodules are prone to occur. Therefore, the aluminum oxide content in the present application is 2.0%-5.0%, which can effectively avoid the above problems.
[0024] At the same time, sulfur-carbon colorant is added in the present invention, which can react with iron ions in the glass to form brown glass with stable color, so that the glass has a better light-shielding effect, meeting the dual requirements of some drugs for chemical resistance and light-shielding.
[0025] The brown medium-boron pharmaceutical glass of the present invention comprises SiO2 introduced from high-purity quartz sand, Al2O3 introduced from calcined alumina and feldspar, B2O3 introduced from chemical raw material borax pentahydrate, Na2O mainly introduced from sodium carbonate and sodium sulfate, K2O mainly introduced from potassium carbonate, CaO introduced from calcium carbonate, and BaO introduced from barium carbonate. The cullet is purchased cullet consistent with the proportion of the components.
[0026] Borax pentahydrate loses its crystal water and part of hydroxyl water at high temperature, thus undergoing a decomposition reaction. As the temperature rises further, the remaining crystal water and hydroxyl water in the decomposition product will continue to evaporate, eventually leaving behind a solid residue with boron oxide as the main component.
[0027] Sodium carbonate and sodium sulfate provide Na2O after heating. Similarly, potassium carbonate, calcium carbonate, and barium carbonate provide K2O, CaO, and BaO respectively after heating.
[0028] SiO2 is one of the main components of glass. It helps to reduce the thermal expansion coefficient of glass and improve the thermal stability, heat resistance, chemical stability and softening temperature of glass. The addition of SiO2 can enhance the network structure of glass and make it denser, thereby resisting the erosion of acidic media. SiO2 forms silicon-oxygen tetrahedrons [SiO4] in glass. These tetrahedrons are interconnected by sharing oxygen atoms to form a continuous three-dimensional network structure. This network structure can effectively block the penetration of H+ ions in acidic media, thereby improving the acid resistance of glass. Reducing the SiO2 content reduces the specific surface area that reacts with alkaline ions. At the same time, by adding other oxides such as alkali metal oxides, the density of glass is increased to form a protective layer or barrier layer, which reduces the direct contact between SiO2 and alkaline ions and enhances the alkali resistance of glass.
[0029] Al2O3 also has a positive effect on the acid resistance of glass. It can form aluminum oxide tetrahedron [AlO4] or other aluminum oxide polyhedrons in the glass. These polyhedrons also participate in the formation of the glass network and help enhance the chemical stability of the glass. The addition of Al2O3 can increase the cationic charge density in the glass network and improve the stability of the network structure. The addition of Al2O3 can increase the cationic charge density in the glass network, help balance the negative charge in the network, reduce the formation of defects and pores, and thus improve the chemical stability of the glass.
[0030] B2O3 plays a dual role as a flux and a network former in glass. It helps to lower the melting temperature of glass and participates in the formation of glass network, improving the chemical stability and resistance to mechanical and thermal shock of glass. B2O3 may form structural units such as boron-oxygen triangles or boron-oxygen tetrahedrons in glass. These units are interconnected with silicon-oxygen tetrahedrons by sharing oxygen atoms to form a more complex network structure. This structure can effectively block the erosion of acidic media and improve the acid resistance of glass.
[0031] Al2O3 and B2O3 may form complex network structures in the glass, which help to resist the corrosion of alkaline media.
[0032] The Na2O, K2O, BaO, and CaO oxides in this application are mainly used as fluxes in glass, which can reduce the melting temperature of glass and promote the formation of glass. These alkali metal and alkaline earth metal oxides are usually present in the form of network exosome ions in glass, which can destroy the continuity of the glass network structure and increase the defects and pores in the glass. These defects and pores may become channels for acidic medium corrosion, thereby reducing the acid resistance of glass. These oxides may exist in the form of network exosome ions in glass, and by adjusting their content and ratio, the compactness, porosity, and surface state of glass can be affected, thereby indirectly affecting the alkali resistance of glass. However, it should be noted that these oxides themselves do not directly improve the alkali resistance of glass, but need to be achieved through the synergistic effect with components such as SiO2, Al2O3, and B2O3.
[0033] In some embodiments, based on the total weight of the medium-boron pharmaceutical glass raw material, the mass percentage of sodium carbonate + potassium carbonate is 3-5%, and / or the mass percentage of barium carbonate + calcium carbonate is 3-5%, and / or the mass percentage of sodium sulfate and carbon powder is 0.7-0.8%.
[0034] Sodium carbonate and potassium carbonate mainly provide Na2O and K2O. Both Na2O and K2O are good fluxing agents that can significantly reduce the melting temperature of glass, making it easier to form glass at a lower temperature. At the same time, they can also reduce the viscosity of the glass liquid and increase the fluidity of the glass liquid, thereby improving the forming properties of the glass. K2O can reduce the crystallization tendency of the glass and increase the transparency and gloss of the glass. Na2O has a great influence on the clarification process of the glass liquid, which helps to remove bubbles and impurities in the glass liquid and improve the quality of the glass. Therefore, a mass percentage of sodium carbonate + potassium carbonate of 3-5% can better optimize the performance of the glass.
[0035] Both barium oxide and calcium oxide can improve the chemical stability of glass to a certain extent. Barium oxide increases the density and refractive index of glass, making it denser and thus resisting the erosion of external chemicals. Calcium oxide, due to its high melting point and hardness, can enhance the corrosion resistance of glass. The two work together to further improve the chemical stability of glass. Barium oxide increases the density and refractive index of glass, making the glass structure denser and reducing the channels and opportunities for erosion by external chemicals. Calcium oxide, due to its high melting point and hardness, can form a protective film on the surface of glass to further resist chemical erosion. The two work together to improve the chemical stability of glass. Barium oxide increases the refractive index and density of glass, making the propagation path of light in the glass more regular and reducing scattering and reflection losses. The high refractive index and low scattering rate of calcium oxide help to improve the light transmittance and clarity of glass. The two complement each other in optical properties, so a mass percentage of barium carbonate + calcium carbonate of 3-5% can optimize glass performance.
[0036] The coloring of brown medium borosilicate glass tubes requires the dual effects of colorant sodium sulfate and reducing agent carbon powder. The addition of sodium sulfate will change the molecular structure of the glass and produce new absorption bands, thereby affecting the propagation and reflection of light in the glass and achieving the coloring effect. In the glass production process, carbon powder as a reducing agent can accelerate the decomposition process of sodium sulfate. Sodium sulfate decomposes at high temperatures to produce gases such as hydrogen sulfide. These gases react with oxides in the glass to help clarify and color the glass. Therefore, the mass percentage of sodium sulfate and carbon powder is 0.7-0.8% to achieve better coloring.
[0037] In some embodiments, based on the total weight of the raw materials for preparing medium-boron medicinal glass, the components of the brown medium-boron medicinal glass include, by mass percentage: 36.0% quartz sand, 3.5% aluminum oxide, 2.0% sodium carbonate, 4.5% feldspar, 13.0% borax, 2.0% potassium carbonate, 2.0% barium carbonate, 2.0% calcium carbonate, 0.3% sodium sulfate, 0.5% carbon powder, and 35% brown broken glass.
[0038] In some embodiments, based on the total weight of the medium-boron pharmaceutical glass raw material, the mass percentage of sodium carbonate + potassium carbonate is 4%, and / or the mass percentage of barium carbonate + calcium carbonate is 4%, and / or the mass percentage of sodium sulfate and carbon powder is 0.8%.
[0039] In some embodiments, the content of silicon dioxide in the quartz sand is greater than 98.5%.
[0040] The second aspect of the present application provides a method for preparing brown medium-boron medicinal glass, which is used for the aforementioned brown medium-boron medicinal glass, comprising the steps of:
[0041] Evenly mix quartz sand, alumina, sodium carbonate, feldspar, borax, potassium carbonate, barium carbonate, calcium carbonate, sodium sulfate, carbon powder and brown broken glass;
[0042] The mixed material is heated to a uniform molten state to obtain a high-quality brown medium-boron medicinal glass liquid;
[0043] The brown medium-boron medicinal glass liquid is drawn into a glass tube of a certain specification;
[0044] The glass tube is roughly cut after it cools down naturally, and then both ends of the glass tube are cut as a whole, and then the final round mouth is made on the end of the glass tube.
[0045] In some embodiments, the uniformity of the mixture is greater than 95%. Uniform batch materials can melt faster because the various raw materials have been fully mixed, reducing the local melting difficulties caused by uneven distribution of raw materials during the melting process. When the batch material uniformity is low, stratification or agglomeration is prone to occur, making it difficult to melt and homogenize the glass, and even causing defects such as streaks and stones in severe cases. Uniform batch materials can effectively avoid these problems and improve the overall quality of the glass.
[0046] In some embodiments, the mixed material heating temperature is 1550° C.-1600° C. Within this temperature range, the glass raw materials can be melted quickly and fully, reducing the melting time and improving production efficiency. High temperature helps to break the chemical bonds in the raw materials and convert them into molten glass liquid.
[0047] In some embodiments, the cooling temperature of the glass tube is 180-220°C.
[0048] In some embodiments, the device for heating and melting the mixed material is a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a mixed heating furnace combining a flame furnace and an all-electric furnace.
[0049] [Example]
[0050] Example 1
[0051] The raw material weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 35.0%, aluminum oxide 5.0%, sodium carbonate 3.0%, feldspar 5.0%, borax 12.0%, potassium carbonate 3.0%, barium carbonate 1.0%, calcium carbonate 1.0%, sodium sulfate 0.2%, carbon powder 0.6%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate used is the proportion of the total batch. Then the forced mixer is used for uniform mixing, and the uniformity reaches more than 95%.
[0052] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0053] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0054] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0055] Example 2
[0056] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 36.0%, alumina 3.5%, sodium carbonate 2.0%, feldspar 4.5%, borax 13.0%, potassium carbonate 2.0%, barium carbonate 2.0%, calcium carbonate 2.0%, sodium sulfate 0.2%, carbon powder 0.6%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0057] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0058] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0059] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0060] Example 3
[0061] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 37.0%, alumina 2.0%, sodium carbonate 1.0%, feldspar 4.0%, borax 14.0%, potassium carbonate 1.0%, barium carbonate 3.0%, calcium carbonate 3.0%, sodium sulfate 0.2%, carbon powder 0.6%, brown broken glass 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then, the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0062] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0063] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0064] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0065] Example 4
[0066] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 35.0%, aluminum oxide 5.0%, sodium carbonate 3.0%, feldspar 5.0%, borax 12.0%, potassium carbonate 3.0%, barium carbonate 1.0%, calcium carbonate 1.0%, sodium sulfate 0.3%, carbon powder 0.5%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate used is the proportion of the total batch. Then the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0067] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0068] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0069] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0070] Example 5
[0071] The raw material weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 36.0%, alumina 3.5%, sodium carbonate 2.0%, feldspar 4.5%, borax 13.0%, potassium carbonate 2.0%, barium carbonate 2.0%, calcium carbonate 2.0%, sodium sulfate 0.3%, carbon powder 0.5%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0072] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0073] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0074] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0075] Example 6
[0076] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 37.0%, alumina 2.0%, sodium carbonate 1.0%, feldspar 4.0%, borax 14.0%, potassium carbonate 1.0%, barium carbonate 3.0%, calcium carbonate 3.0%, sodium sulfate 0.3%, carbon powder 0.5%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0077] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0078] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0079] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0080] Example 7
[0081] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 35.0%, aluminum oxide 5.0%, sodium carbonate 3.0%, feldspar 5.0%, borax 12.0%, potassium carbonate 3.0%, barium carbonate 1.0%, calcium carbonate 1.0%, sodium sulfate 0.4%, carbon powder 0.4%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then, the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0082] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0083] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0084] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0085] Example 8
[0086] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 36.0%, alumina 3.5%, sodium carbonate 2.0%, feldspar 4.5%, borax 13.0%, potassium carbonate 2.0%, barium carbonate 2.0%, calcium carbonate 2.0%, sodium sulfate 0.4%, carbon powder 0.4%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then, the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0087] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0088] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0089] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0090] Example 9
[0091] The raw materials weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 37.0%, alumina 2.0%, sodium carbonate 1.0%, feldspar 4.0%, borax 14.0%, potassium carbonate 1.0%, barium carbonate 3.0%, calcium carbonate 3.0%, sodium sulfate 0.4%, carbon powder 0.4%, brown cullet 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then the materials are evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0092] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0093] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0094] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0095] Comparative Example 1
[0096] The raw material weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 36.0%, alumina 3.5%, sodium carbonate 2.0%, feldspar 4.5%, borax 13.0%, potassium carbonate 2.0%, barium carbonate 2.0%, calcium carbonate 2.0%, no sodium sulfate, carbon powder 0.6%, brown broken glass 35.0%. The amount of carbon powder and sodium sulfate is the proportion of the total batch. Then the forced mixer is used for uniform mixing, and the uniformity reaches more than 95%.
[0097] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0098] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0099] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0100] Comparative Example 2
[0101] The raw material weight ratio of brown medium-boron pharmaceutical glass is: quartz sand 36.0%, alumina 3.5%, sodium carbonate 2.0%, feldspar 4.5%, borax 13.0%, potassium carbonate 2.0%, barium carbonate 2.0%, calcium carbonate 2.0%, sodium sulfate 0.4%, no carbon powder, brown cullet 35.0%. Among them, the amount of carbon powder and sodium sulfate used is the proportion of the total batch. Then it is evenly mixed in a forced mixer, and the uniformity reaches more than 95%.
[0102] Add the batch materials into a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a combined heating furnace, preferably an all-electric glass melting furnace. Make the temperature of the mixture reach 1550℃-1600℃, make the mixture reach a uniform melting state, and obtain high-quality brown medium-boron medicinal glass liquid.
[0103] The high-quality and qualified glass liquid is sent to the molding equipment, which can be the Veloce method or the Danner molding method, and drawn into a glass tube of a certain specification.
[0104] When the glass tube passes through the runway and is naturally cooled to about 200℃, it passes through the rough cutting knife of the traction machine and is roughly cut into the required length. Then, the two ends of the glass tube are cut as a whole through fine cutting, and the ends of the glass tube are finally rounded with a flame, so that the ends of the glass tube are smooth, easy to pack and safe to carry.
[0105] Table 1 Raw material composition table of Examples 1-9
[0106]
[0107] Table 2 Raw material composition table of comparative examples 1-7
[0108]
[0109] Table 3 Test performance of Examples 1-9
[0110]
[0111] Table 4 Test performance of comparative examples 1-7
[0112]
[0113] Comparative Example 1 uses sodium sulfate without colorant and only adds reducing agent carbon powder, while Comparative Example 2 uses carbon powder without reducing agent and only adds sodium sulfate as colorant. The brown neutral borosilicate glass obtained in Comparative Examples 1 and 2 fails to form effective coloring of the glass tube compared with the brown neutral borosilicate glass of Examples 1-9. In other words, the coloring of the brown neutral borosilicate glass tube requires the dual effects of the colorant sodium sulfate and the reducing agent carbon powder. At the same time, it was also found in production that the products in the comparative examples had more gas-deficient line defects. In other words, the use of one additive raw material is not conducive to production, and the inappropriate proportion used will affect the stability of the coloring of the glass tube.
[0114] In comparative example 3, when the content of sodium carbonate + potassium carbonate is greater than 6%, the expansion coefficient becomes significantly larger and the acid resistance becomes worse; in comparative example 4, when the content of sodium carbonate + potassium carbonate is less than 3%, and in comparative example 5, when the content of barium carbonate + calcium carbonate is less than 3%, the performance of the two is relatively similar, and the expansion coefficient performance is better, but the glass tube hot forming process becomes difficult, which seriously affects the batch stable industrial production of glass tubes; in comparative example 6, when the content of barium carbonate + calcium carbonate is greater than 5%, the glass is formed due to the material properties of the glass liquid becoming shorter. The specifications and dimensions of the glass tube forming process are difficult to control, which has a certain impact on production; in comparative example 7, when the content of sodium sulfate + carbon powder is greater than 0.8%, the gas line defects on the glass tube in glass production are very high, which seriously affects the industrial production yield.
[0115] It can be seen from Table 1 and Table 3 that the expansion coefficients of the brown neutral borosilicate glass of the three groups of Examples 1-3, Examples 4-6, and Examples 6-9 are in the range of 53-51×10 -7 / K, the acid resistance is level one, and the alkali resistance is level two. They all meet the needs of medium-boron pharmaceutical glass, but the color of the glass tube varies between light yellow and brownish yellow. At the same time, the samples were scanned with ultraviolet light of 290 to 450 nm and visible light of 590 to 610 nm, and the light transmittance of the samples was compared with that of the preferred embodiment 5. When the addition amount of the colorant sodium sulfate was 0.3% and the addition amount of the carbon powder was 0.5%, the coloring was relatively stable and the shading effect was good.
[0116] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A brown medium-boron medicinal glass, characterized in that: Based on the total weight of the raw materials for preparing medium-boron medicinal glass, the components of the brown medium-boron medicinal glass include, by mass percentage, 35.0%-37.0% quartz sand, 2.0%-5.0% alumina, 1.0%-3.0% sodium carbonate, 6.0%-2.0% feldspar, 12.0%-14.0% borax, 1.0%-3.0% potassium carbonate, 3.0%-1.0% barium carbonate, 1.0%-3.0% calcium carbonate, 0.4%-0.1% sodium sulfate, 0.1%-0.6% carbon powder and 35.0% brown broken glass.
2. The brown medium-boron medicinal glass according to claim 1, characterized in that: Based on the total weight of the medium-boron medicinal glass raw material, the mass percentage of the sodium carbonate + potassium carbonate is 3-5%, and / or the mass percentage of barium carbonate + calcium carbonate is 3-5%, and / or the mass percentage of sodium sulfate + carbon powder is 0.7-0.8%.
3. The brown medium-boron medicinal glass according to claim 1, characterized in that: Based on the total weight of the raw materials for preparing medium-boron medicinal glass, the components of the brown medium-boron medicinal glass include, by mass percentage, 36.0% quartz sand, 3.5% aluminum oxide, 2.0% sodium carbonate, 4.5% feldspar, 13.0% borax, 2.0% potassium carbonate, 2.0% barium carbonate, 2.0% calcium carbonate, 0.3% sodium sulfate, 0.5% carbon powder, and 35% brown broken glass.
4. The brown medium-boron medicinal glass according to claim 1, characterized in that: Based on the total weight of the medium-boron medicinal glass raw material, the mass percentage of sodium carbonate + potassium carbonate is 4%, and / or the mass percentage of barium carbonate + calcium carbonate is 4%, and / or the mass percentage of sodium sulfate and carbon powder is 0.8%.
5. The brown medium-boron medicinal glass according to claim 1, characterized in that: The content of silicon dioxide in the quartz sand is greater than 98.5%.
6. A method for preparing brown medium-boron medicinal glass, for preparing the brown medium-boron medicinal glass according to any one of claims 1 to 4, characterized in that: Includes steps: Evenly mix quartz sand, alumina, sodium carbonate, feldspar, borax, potassium carbonate, barium carbonate, calcium carbonate, sodium sulfate, carbon powder and brown broken glass; The mixed material is heated to a uniform molten state to obtain a high-quality brown medium-boron medicinal glass liquid; The brown medium-boron medicinal glass liquid is drawn into a glass tube of a certain specification; The glass tube is roughly cut after it cools down naturally, and then both ends of the glass tube are cut as a whole, and then the final round mouth is made on the end of the glass tube.
7. The method for preparing brown medium-boron medicinal glass according to claim 6, characterized in that: The mixing uniformity is greater than 95%.
8. The method for preparing brown medium-boron medicinal glass according to claim 6, characterized in that: The mixing material heating temperature is 1550°C-1600°C.
9. The method for preparing brown medium-boron medicinal glass according to claim 6, characterized in that: The cooling temperature of the glass tube is 180-220°C.
10. The method for preparing brown medium-boron medicinal glass according to claim 6, characterized in that: The equipment for heating and melting the mixed materials is a glass melting furnace, which can be a flame furnace, an all-electric furnace, or a mixed heating furnace combining a flame furnace and an all-electric furnace.
Citation Information
Patent Citations
Formulation for medicinal neutral boron silicate glass
CN101148317A
First grade water-fast pharmaceutical glass tube and preparation method
CN104926127A
All-electric melting brown medicinal glass and preparation method thereof
CN116119922A
Medicinal soda-lime glass tube and preparation process thereof
CN116119926A
Brown medicinal neutral borosilicate glass tube and preparation method thereof
CN118373592A