Preparation method of artificial gem-containing solid waste zirconium material ultra-white cover glaze
Through the specific ratio and firing process of artificial gem solid waste zirconium materials and other ceramic materials, low-cost, low radioactivity, high whiteness and wear resistance are prepared, which solves the zirconium silicate increase in the prior art The high cost of whitening agents and radioactive risks have achieved the purpose of resource conservation and environmentally friendly.
Patent Information
- Application Number
- CN202411128607.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, zirconium silicate is used as a whitening agent in building ceramics with high cost and radioactive risks. It has not yet been used to make ultra-white glaze with artificial gem solid waste zirconium material.
Using the specific ratio of artificial gem solid waste zirconium materials to sodium feldspar, potassium feldspar, quartz, kaolin, calcium, calcium, calcium, calcium, barium carbonate and ultra-white alumina, ultra-white glaze is prepared through ball milling and firing processes. , the amount of zirconium used in artificial gemstone solid waste is controlled to be 5 to 10% to improve the whiteness and wear resistance of the glaze surface.
It has achieved low-cost, low-radioactive, high whiteness and good color ultra-white glaze, which meets the usage standards, realizes the recycling of waste resources, reduces production costs, and improves the wear resistance and stability of the glaze.
Smart Images

Figure BDA0004997180230000061 
Figure BDA0004997180230000071 
Figure BDA0004997180230000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building ceramics, and in particular to a method for preparing an ultra-white glaze containing artificial gemstone solid waste zirconium material. Background Art
[0002] Artificial gemstone solid waste zirconium materials refer to zirconium-containing wastes generated during the production and processing of artificial gemstones, especially synthetic cubic zirconia (CZ) and its related by-products. These wastes usually contain zirconium oxide (ZrO2), yttrium oxide (Y2O3), calcium oxide (CaO), silicates, aluminum oxide (Al2O3), iron (Fe), manganese (Mn) and other components. Further recycling of these wastes can reduce environmental pollution and enhance their value.
[0003] When producing porcelain tile products, a common ceramic opacifier zirconium silicate is usually added to the glaze. After the ceramic glaze is fired, zirconium silicate will form baddeleyite, which scatters the incident light to achieve the effect of visual opacification and whitening. Usually, zirconium silicate in building ceramics comes from zircon sand. According to the needs, the whiteness of the glaze is usually controlled at about 70 degrees. The amount of zirconium silicate added is often 10% to 15%, and the usage is very large; the current market price of zirconium silicate is 20,000 yuan / ton. When added at 10-15%, the cost of zirconium silicate is 2,000 to 3,000 yuan / ton, which accounts for a very high cost of the glaze. Therefore, it is urgent to develop an ultra-white glaze containing artificial gemstone solid waste zirconium material. Through the utilization of solid waste, not only can the production cost be reduced, but also the waste resources can be recycled to achieve the purpose of resource conservation and environmental friendliness.
[0004] In the prior art, the preparation method of ultra-white glaze is mainly as follows:
[0005] Patent "A Process for Preparing Ultra-White Glaze" application number: 202010026707.5 uses high-white potassium feldspar and sodium feldspar in combination with zirconium silicate to achieve the effect of increasing whiteness. The melting temperature of potassium feldspar is not high and the melting temperature range is wide, but the high-temperature viscosity is large and bubbles are difficult to discharge. The melting temperature of sodium feldspar is low, and no new crystal phase is produced during melting. The formed liquid phase has low viscosity and a narrow melting range, which is not conducive to a low-temperature fast burning environment. The high-white potassium feldspar and high-white sodium feldspar used in the patent simply increase the purity of ordinary high-potassium feldspar and sodium feldspar, reduce the Fe and Ti impurity content, and thus improve whiteness.
[0006] Patent "A Ceramic Ultra-white Glaze" application number: 201811514587.2 uses a combination of zirconium silicate, cerium dioxide and yttrium aluminate as an emulsifier to achieve a whitening effect. The whiteness of the glaze is relatively high, but the radioactivity is also increased. Multiple emulsifiers are used at the same time. These emulsifiers are all radioactive, and the two oxides are toxic in themselves, which increases the difficulty of operation and the risk during storage. Yttrium aluminate is expensive, and the overall cost is higher than that of ordinary porcelain tile glaze.
[0007] Patent "A glaze and its preparation method, glazed tile" application number: 202210924943.8 uses high-white alumina to completely replace the original alumina, and is used with zirconium silicate to achieve a whitening effect. However, when too much high-white alumina is added, the color of the glaze will be relatively poor.
[0008] The above methods all directly use zirconium silicate for whitening, which makes the production cost too high and brings radioactive risks to the home environment. At present, there is no report on the use of artificial gemstone solid waste zirconium materials to make ultra-white glaze. In order to process and use artificial gemstone solid waste zirconium materials, the applicant has experimentally explored the effects of different proportions of albite, potassium feldspar, nepheline, ultra-white alumina, quartz, kaolin, calcined talc, barium carbonate, etc. on whiteness, as well as the effect of increasing the ultra-white alumina content on the whiteness of the glaze, and realized the effective use of artificial gemstone solid waste zirconium materials in ultra-white glaze. Summary of the invention
[0009] In view of the above shortcomings, the present invention provides a method for preparing an ultra-white glaze containing artificial gemstone solid waste zirconium material, which solves the problem that artificial gemstone solid waste zirconium material has not yet been used to make ultra-white glaze. The glaze made of artificial gemstone solid waste zirconium material has high whiteness, good color and high wear resistance. The specific technical scheme is as follows:
[0010] An ultra-white glaze containing artificial gemstone solid waste zirconium material, comprising the following raw materials in parts by weight: 0-32 parts of albite, 0-32 parts of potassium feldspar, 13-19 parts of quartz, 13-16 parts of nepheline, 7-10 parts of kaolin, 5-8 parts of calcined kaolin, 1-3 parts of burned talc, 1-3 parts of barium carbonate, 10-16 parts of ultra-white alumina and 5-10 parts of artificial gemstone solid waste zirconium.
[0011] Preferably, an ultra-white glaze containing artificial gem solid waste zirconium material includes the following raw materials in parts by weight: 16-32 parts of albite, 0-16 parts of potassium feldspar, 13-15 parts of quartz, 13-14 parts of nepheline, 7-9 parts of kaolin, 5-7 parts of calcined kaolin, 1-2 parts of burned talc, 2-3 parts of barium carbonate, 14-16 parts of ultra-white alumina and 7-10 parts of artificial gem solid waste zirconium.
[0012] Furthermore, the usage of the artificial gemstone solid waste zirconium in the ultra-white glaze containing the artificial gemstone solid waste zirconium material is controlled at 5wt% to 10wt%.
[0013] Furthermore, the glaze whiteness of the ceramic product made from the ultra-white glaze containing artificial gemstone solid waste zirconium material is 71 to 72 degrees.
[0014] Furthermore, the ultra-white glaze raw materials include the following chemical components by weight percentage: SiO2: 54-57%, Al2O3: 33-35%, BaCO3: 1-2.5%, MgO: 1-2%, K2O: 1-1.5%, Na2O: 3-5%, ZrO2: 3-4.5%, and loss on ignition: 1-2.5%.
[0015] The present invention also provides a method for preparing an ultra-white glaze containing artificial gemstone solid waste zirconium material, the method comprising the following steps:
[0016] (1) Weigh each raw material by weight;
[0017] (2) mixing the raw materials, adding water, carboxymethyl cellulose and sodium tripolyphosphate and ball-milling together, and controlling the fineness to be 0.4-0.6% of the residue after passing through a 325-mesh sieve to obtain a mixed material;
[0018] (3) The mixture is aged for 18 to 24 hours to obtain an ultra-white glaze containing artificial gemstone solid waste zirconium material to be used, and the ultra-white glaze containing artificial gemstone solid waste zirconium material to be used is evenly poured on the brick blank using a bell jar and fired, thereby completing the application of the ultra-white glaze.
[0019] Furthermore, in step (2), the raw materials are mixed, 38% of water, 0.13% of carboxymethyl cellulose and 0.3% of sodium tripolyphosphate are added and ball-milled together, and the fineness is controlled to be 0.4-0.6% after passing through a 325-mesh sieve to obtain a mixture.
[0020] Furthermore, in step (3), the mixture is aged for 18 to 24 hours, the specific gravity is controlled at 1.83 to 1.88, and the flow rate is controlled at 26 to 30 seconds to obtain an ultra-white glaze containing artificial gemstone solid waste zirconium material.
[0021] Furthermore, in step (3), the sintering temperature is 1140-1160° C., and the sintering time is 40-50 min.
[0022] Mechanism: Alumina is in the silicon-oxygen grid of glass in the mortar, which can increase the viscosity of the glaze, reduce the solubility of zircon, and make the crystal grains no longer melt and participate in the solid-phase emulsification behavior in the form of residual crystal phase. The aluminum-oxygen tetrahedral network structure formed by the introduction of alumina will inhibit the diffusion and migration of Si4+, thereby affecting the combination of Si and Zr to form zirconium silicate crystals, which can inhibit the dissolution of zircon and is conducive to the emulsification of zirconium silicate, thereby improving whiteness. However, with the increase of aluminum content, the firing temperature of the glaze will also increase. Magnesium oxide forms a liquid phase at a lower temperature, which can reduce the firing temperature, improve thermal stability, and widen the melting range. Therefore, the addition of talc can reduce the firing temperature of the glaze. Barium carbonate can improve the color and stabilize the gloss of the glaze and improve the wear resistance of the glaze, so an appropriate amount of barium carbonate is used in the formula.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention innovatively uses artificial gemstone solid waste zirconium materials to prepare glazes. Only 5-10% of artificial gemstone solid waste zirconium materials can be used to prepare glazes with high whiteness, good color and high wear resistance, which meets the use standards, realizes the recycling of waste resources, reduces production costs, and achieves the purpose of resource conservation and environmental friendliness.
[0025] 2. The present invention achieves enhanced effect on the whiteness of the glaze by newly adding ultra-white alumina. When the ultra-white alumina content is too much, the color is poor. Adding barium carbonate improves the color, stabilizes the color and glossiness, and improves the wear resistance of the glaze.
[0026] 3. The present invention increases the content of alumina, increases the viscosity of the glaze, reduces the solubility of zircon, and makes the crystal grains no longer melt and participate in the solid phase opacification behavior in the form of residual crystal phase, thereby increasing the whiteness of the surface glaze. By adding an appropriate amount of talc, the firing temperature of the surface glaze can be adjusted, and the roughness of the glaze surface can be improved. By adjusting the ratio of sodium feldspar and potassium feldspar, the firing temperature of the glaze surface can be controlled, thereby stabilizing the production. DETAILED DESCRIPTION
[0027] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0028] Example 1
[0029] The specific ingredients by weight are as follows:
[0030] 32 parts of sodium feldspar, 0 parts of potassium feldspar, 13 parts of quartz, 13 parts of nepheline, 7 parts of kaolin, 5 parts of calcined kaolin, 2 parts of burned talc, 2 parts of barium carbonate, 16 parts of ultra-white alumina, and 10 parts of artificial gemstone solid waste zirconium.
[0031] The chemical composition is as follows: SiO2: 54%, Al2O3: 33%, BaCO3: 2.5%, MgO: 1%, K2O: 1%, Na2O: 3%, ZrO2: 3%, loss on ignition: 2.5%.
[0032] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.4% (325 mesh sieve), age for 18 hours, control the specific gravity to 1.83, control the flow rate to 26 seconds, use a bell jar to evenly pour glaze on the brick, and fire it at a firing temperature of 1140°C and a firing time of 40 minutes. Measure the whiteness and LAB value, glossiness, and dirt absorption, and observe the glaze condition.
[0033] Example 2
[0034] The specific ingredients by weight are as follows:
[0035] 23 parts of sodium feldspar, 9 parts of potassium feldspar, 13 parts of quartz, 13 parts of nepheline, 7 parts of kaolin, 5 parts of calcined kaolin, 2 parts of burned talc, 2 parts of barium carbonate, 16 parts of ultra-white alumina, and 10 parts of artificial gemstone solid waste zirconium.
[0036] The chemical composition is as follows: SiO2: 47%, Al2O3: 35%, BaCO3: 2.5%, MgO: 2%, K2O: 1.5%, Na2O: 5%, ZrO2: 4.5%, loss on ignition: 2.5%.
[0037] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.6% (325 mesh sieve), age for 24 hours, control the specific gravity to 1.88, control the flow rate to 30 seconds, use a bell jar to evenly pour glaze on the brick, and fire it at a firing temperature of 1160°C and a firing time of 50 minutes. Measure the whiteness and LAB value, glossiness, and dirt absorption, and observe the glaze condition.
[0038] Example 3
[0039] The specific ingredients by weight are as follows:
[0040] 9 parts of sodium feldspar, 23 parts of potassium feldspar, 13 parts of quartz, 13 parts of nepheline, 7 parts of kaolin, 5 parts of calcined kaolin, 2 parts of burned talc, 2 parts of barium carbonate, 16 parts of ultra-white alumina, and 10 parts of artificial gemstone solid waste zirconium.
[0041] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.4% (325 mesh sieve), age for 24 hours, control the specific gravity to 1.83, control the flow rate to 30 seconds, use a bell jar to evenly pour glaze on the brick, and fire it at a firing temperature of 1140°C and a firing time of 50 minutes. Measure the whiteness and LAB value, glossiness, and dirt absorption, and observe the glaze condition.
[0042] Example 4
[0043] The specific ingredients by weight are as follows:
[0044] 0 parts of sodium feldspar, 32 parts of potassium feldspar, 13 parts of quartz, 13 parts of nepheline, 7 parts of kaolin, 5 parts of calcined kaolin, 2 parts of burned talc, 2 parts of barium carbonate, 16 parts of ultra-white alumina, and 10 parts of artificial gemstone solid waste zirconium.
[0045] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.4% (325 mesh sieve), age for 24 hours, control the specific gravity to 1.83, control the flow rate to 30 seconds, use a bell jar to evenly pour glaze on the brick, and fire it at a firing temperature of 1140°C and a firing time of 50 minutes. Measure the whiteness and LAB value, glossiness, and dirt absorption, and observe the glaze condition.
[0046] Example 5
[0047] The specific ingredients by weight are as follows:
[0048] 16 parts of sodium feldspar, 16 parts of potassium feldspar, 13 parts of quartz, 13 parts of nepheline, 7 parts of kaolin, 5 parts of calcined kaolin, 1 part of burned talc, 3 parts of barium carbonate, 16 parts of ultra-white alumina, and 10 parts of artificial gemstone solid waste zirconium.
[0049] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.6% (325 mesh sieve), age for 24 hours, control the specific gravity to 1.88, control the flow rate to 30 seconds, use a bell jar to evenly pour glaze on the brick, and fire it at a firing temperature of 1160°C and a firing time of 50 minutes. Measure the whiteness and LAB value, glossiness, and dirt absorption, and observe the glaze condition.
[0050] Example 6
[0051] The specific ingredients by weight are as follows:
[0052] 16 parts of sodium feldspar, 16 parts of potassium feldspar, 13 parts of quartz, 13 parts of nepheline, 7 parts of kaolin, 5 parts of calcined kaolin, 3 parts of burned talc, 1 part of barium carbonate, 16 parts of ultra-white alumina, and 10 parts of artificial gemstone solid waste zirconium.
[0053] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.6% (325 mesh sieve), age for 24 hours, control the specific gravity to 1.88, control the flow rate to 30 seconds, use a bell jar to evenly pour glaze on the brick, and fire it at a firing temperature of 1160°C and a firing time of 50 minutes. Measure the whiteness and LAB value, glossiness, and dirt absorption, and observe the glaze condition.
[0054] Example 7
[0055] The specific ingredients by weight are as follows:
[0056] 10 parts of sodium feldspar, 16 parts of potassium feldspar, 19 parts of quartz, 16 parts of nepheline, 10 parts of kaolin, 8 parts of calcined kaolin, 3 parts of burned talc, 3 parts of barium carbonate, 10 parts of ultra-white alumina, and 5 parts of artificial gemstone solid waste zirconium.
[0057] The chemical components of Examples 3 to 7 are as follows: SiO2: 54.3%, Al2O3: 33.2%, BaCO3: 1.35%, MgO: 1.98%, K2O: 1.38%, Na2O: 3.56%, ZrO2: 3.32%, and loss on ignition: 1.91%.
[0058] Preparation method: Mix the required raw materials in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, 0.3% sodium tripolyphosphate, control the fineness of the balls to 0.5% (325 mesh sieve), age for 20 hours, control the specific gravity to 1.85, control the flow rate to 29 seconds, use a bell jar to evenly pour the glaze on the brick, and burn it at a firing temperature of 1150°C and a firing time of 45 minutes. Measure the whiteness and LAB value, glossiness, dirt absorption, and observe the glaze surface. The whiteness detection results of each embodiment are shown in Table 1:
[0059] Table 1:
[0060] project Whiteness Blue 50 grayscale LAB value Yellow 50 grayscale LAB value Red 50 grayscale LAB value Example 1 72 49.12-8.28-31.17 84.96-3.59 26.18 67.94 23.85 20.68 Example 2 72 49.67-8.04-28.93 84.65-3.37 23.62 70.43 18.61 18.22 Example 3 71 49.76-8.32-29.66 84.77-3.48 25.74 68.08 22.47 19.54 Example 4 71 49.43-8.15-28.75 84.79-3.46 23.42 70.58 18.79 18.73 Example 5 72 49.84-8.35-31.29 84.85-3.46 26.57 67.81 23.13 20.53 Example 6 71 49.81-8.49-29.82 84.78-3.47 25.66 68.25 22.49 19.67 Example 7 71 49.75-8.41-27.56 84.69-3.51 26.71 67.33 21.52 19.41
[0061] The radioactivity and whiteness comparison between the glaze of the present invention and the glaze of the prior art is shown in Table 2:
[0062] Table 2:
[0063] It can be seen that the existing glazes add whitening agents such as zirconium silicate or other radioactive opacifiers, which bring radioactive risks to the home environment. However, the glaze of the present invention has the characteristics of low radioactivity and excellent whiteness.
[0064] Comparative Example 1
[0065] This comparative example does not contain ultra-white alumina, and other component proportions and preparation methods are the same as those of Example 5.
[0066] Comparative Example 2
[0067] The ultra-white alumina in this comparative example is 20 parts, and the other component proportions and preparation methods are the same as those in Example 5.
[0068] Comparative Example 3
[0069] This comparative example does not contain barium carbonate, and the other component proportions and preparation methods are the same as those of Example 5.
[0070] Comparative Example 4
[0071] The barium carbonate in this comparative example is 5 parts, and the other component proportions and preparation methods are the same as those in Example 5.
[0072] The glazes of Example 5 and Comparative Examples 1 to 4 were used to make glazed tiles, and the performance of the glazed tiles was tested (the thickness of the product was 8 mm). The preparation of the glazed tiles is as follows: the raw materials are mixed evenly according to the proportion, put into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, 0.3% sodium tripolyphosphate, the ball fineness is controlled at 0.6% (325 mesh sieve), aged for 24 hours, the specific gravity is controlled at 1.88, the flow rate is controlled at 30 seconds, and the glaze is evenly poured on the brick blank using a bell jar, and fired at a firing temperature of 1160°C and a firing time of 50 minutes. The performance of each glazed tile was tested, and the results are shown in Table 3:
[0073] Table 3:
[0074] project Antifouling performance Wear resistance Glossiness Whiteness Example 5 A-level Level 5 36 72 Comparative Example 1 Class B Level 5 35 62 Comparative Example 2 Class B Level 5 35 64 Comparative Example 3 Class B Level 3 36 71 Comparative Example 4 Class B Level 3 32 71
[0075] The table shows that ultra-white alumina and its proportion (10-16 parts) will affect the whiteness of the glaze. The present invention adds ultra-white alumina and adjusts the appropriate proportion to achieve an enhanced effect on the whiteness of the glaze. Barium carbonate and its proportion will affect wear resistance. The present invention adds barium carbonate and adjusts the appropriate proportion (1-3 parts) to improve color development, stabilize color and gloss, and improve the wear resistance of the glaze.
[0076] In order to illustrate that the present invention can reduce costs, the following cost comparison is made, see Table 4:
[0077] Table 4:
[0078]
[0079]
[0080] In summary, the present invention pioneered the use of artificial gemstone solid waste zirconium materials to prepare glazes. Only 5-10% of artificial gemstone solid waste zirconium materials can be used to prepare glazes with high whiteness, good color and high wear resistance, which meets the use standards, realizes the recycling of waste resources, reduces production costs, and achieves the purpose of resource conservation and environmental friendliness. At the same time, the present invention achieves an enhanced effect on the whiteness of the glaze by newly adding ultra-white alumina. When the ultra-white alumina content is too much, the color is poor. Adding barium carbonate improves the color, stabilizes the color and gloss, and improves the wear resistance of the glaze. In addition, the alumina content is increased, the viscosity of the glaze is increased, the solubility of zircon is reduced, and the crystal grains of crystallization are no longer melted to participate in the solid phase opacification behavior in the form of residual crystal phase, thereby increasing the whiteness of the glaze. By adding an appropriate amount of talc, the firing temperature of the glaze can be adjusted, and the roughness of the glaze surface can be improved. The firing temperature of the glaze surface can be controlled by adjusting the ratio of sodium feldspar and potassium feldspar, so that the production is stable.
[0081] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. An ultra-white glaze containing artificial gemstone solid waste zirconium material, characterized in that: The invention comprises the following raw materials in parts by weight: 0-32 parts of albite, 0-32 parts of potassium feldspar, 13-19 parts of quartz, 13-16 parts of nepheline, 7-10 parts of kaolin, 5-8 parts of calcined kaolin, 1-3 parts of burned talc, 1-3 parts of barium carbonate, 10-16 parts of ultra-white alumina and 5-10 parts of artificial gemstone solid waste zirconium.
2. The ultra-white glaze made of solid waste zirconium material containing artificial gemstones according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 16-32 parts of albite, 0-16 parts of potassium feldspar, 13-15 parts of quartz, 13-14 parts of nepheline, 7-9 parts of kaolin, 5-7 parts of calcined kaolin, 1-2 parts of burned talc, 2-3 parts of barium carbonate, 14-16 parts of ultra-white alumina and 7-10 parts of artificial gemstone solid waste zirconium.
3. The ultra-white glaze made of solid waste zirconium material containing artificial gemstones according to any one of claims 1 or 2, characterized in that: The amount of the artificial gemstone solid waste zirconium in the ultra-white glaze containing the artificial gemstone solid waste zirconium material is controlled to be 5wt% to 10wt%.
4. The ultra-white glaze made of solid waste zirconium material containing artificial gemstones according to any one of claims 1 or 2, characterized in that: The glaze whiteness of the ceramic product made from the ultra-white glaze containing artificial gemstone solid waste zirconium material is 71 to 72 degrees.
5. The ultra-white glaze made of solid waste zirconium material containing artificial gemstones according to any one of claims 1 or 2, characterized in that: The ultra-white glaze raw materials include the following chemical components by weight percentage: SiO2: 54-57%, Al2O3: 33-35%, BaCO3: 1-2.5%, MgO: 1-2%, K2O: 1-1.5%, Na2O: 3-5%, ZrO2: 3-4.5%, and loss on ignition: 1-2.5%.
6. A method for preparing an ultra-white glaze made of solid waste zirconium material containing artificial gemstones according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) Weigh each raw material by weight; (2) mixing the raw materials, adding water, carboxymethyl cellulose and sodium tripolyphosphate and ball-milling together, and controlling the fineness to be 0.4-0.6% of the residue after passing through a 325-mesh sieve to obtain a mixed material; (3) The mixture is aged for 18 to 24 hours to obtain an ultra-white glaze containing artificial gemstone solid waste zirconium material to be used, and the ultra-white glaze containing artificial gemstone solid waste zirconium material to be used is evenly poured on the brick blank using a bell jar and fired, thereby completing the application of the ultra-white glaze.
7. The method for preparing an ultra-white glaze containing artificial gemstone solid waste zirconium material according to claim 6, characterized in that: In step (2), the raw materials are mixed, 38 wt% of water, 0.13 wt% of carboxymethyl cellulose and 0.3 wt% of sodium tripolyphosphate are added and ball-milled together, and the fineness is controlled to be 0.4-0.6% after passing through a 325 mesh sieve to obtain a mixture.
8. The method for preparing an ultra-white glaze containing artificial gemstone solid waste zirconium material according to claim 6, characterized in that: In step (3), the mixture is aged for 18 to 24 hours, the specific gravity is controlled at 1.83 to 1.88, and the flow rate is controlled at 26 to 30 seconds to obtain an ultra-white glaze containing artificial gemstone solid waste zirconium material.
9. The method for preparing an ultra-white glaze containing artificial gemstone solid waste zirconium material according to claim 6, characterized in that: In step (3), the sintering temperature is 1140-1160° C., and the sintering time is 40-50 min.
Citation Information
Patent Citations
Ceramic super-white overglaze
CN109553301A
Preparation process of super-white surface glaze
CN111196679A
Overglaze, preparation method thereof and glazed tile
CN114956566A
Method for preparing zirconium silicate powder by using zirconium-containing waste
CN107572821A
Emulsion glaze and its products made from zirconium dioxide leavings
CN1096023A
Cited By
Method for improving wear resistance of porcelain glazed brick by using artificial gemstone solid waste
CN119430654A
Method for preparing high-performance architectural ceramic tiles using artificial gemstone processing solid waste
CN122771736A