Alkali-free glass fiber and preparation method thereof

Through the combination of SiO2-Al2O3-MgO-CaO mesh structure and praseodymium oxide, combined with the wetting agent of epoxy resin and phenolic resin, high-temperature melting and continuous heat treatment technology, the existing glass fibers are easily corroded under high temperature and high humidity conditions. In the problem, alkali-free glass fibers with high temperature resistance, chemical stability and excellent electrical insulation performance were prepared.

CN118993553APending Publication Date: 2024-11-22徐州志正装饰材料有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411245981.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing glass fibers are prone to corrosion and damage under high temperature and high humidity conditions, and the use of alkaline chemicals during the preparation process does not conform to the concept of sustainable development, and lacks alkaline-free glass fibers with excellent high temperature resistance, chemical stability and electrical insulation performance.

Method used

The mesh-shaped glass fiber consisting of SiO2-Al2O3-MgO-CaO is added to improve stability. During the preparation process, epoxy resin, phenolic resin and antioxidant are used as wetting agents, and high-temperature melting and continuous heat treatment process are used. Prepare alkali-free glass fibers.

Benefits of technology

The prepared alkali-free glass fiber has high tensile strength, low coefficient of expansion, excellent electrical insulation properties and chemical stability. It is suitable for the manufacture of electrical insulation materials and is not prone to corrosion and damage under high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005030746330000071
    Figure BDA0005030746330000071
Patent Text Reader

Abstract

The invention relates to the technical field of glass fibers, in particular to an alkali-free glass fiber and a preparation method thereof. The invention provides an alkali-free material. The alkali-free material comprises the following raw materials: 45-60% of silicon dioxide; 20-30% of aluminum oxide; 1-3% of magnesium oxide; 1.5-2% of calcium oxide; 0.01 to 0.05 percent of praseodymium oxide; 2-3% of an impregnating compound; and 1-1.5% of an antioxidant. The preparation method comprises the following steps: S1, preparing molten glass; the preparation method comprises the following three steps: S1, preparing alkali-free glass fibers, S2, cooling and wiredrawing, and S3, preparing the alkali-free glass fibers, and the step of continuous heat treatment is added in the step of preparing the alkali-free glass fibers in the step S3, so that the friction coefficient between internal structures of the glass fibers becomes smaller, and the shaping effect of a finished product is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass fibers, and in particular to an alkali-free glass fiber and a preparation method thereof. Background Art

[0002] Glass fiber is made from raw materials such as glass balls or waste glass through high-temperature melting and drawing processes. It is an inorganic non-metallic material with excellent performance.

[0003] Alkali-free glass fiber refers to glass fiber with an alkali metal oxide content of less than 0.8%. Compared with ordinary glass fiber, alkali-free glass fiber has higher high temperature resistance, high tensile strength and small elongation, and maintains a stable shape and size; it has good chemical stability and is not easy to corrode and break under harsh conditions such as high temperature and high humidity; it has excellent electrical insulation properties and is suitable for the manufacture of electrical insulation materials; it has good processing performance. Alkali-free glass fiber is widely used in aerospace, automobile manufacturing, building materials, electronics industry and other fields. At the same time, since alkali-free glass fiber does not use alkaline chemicals in the preparation process, it is more in line with the sustainable development concept of modern society. Therefore, it is necessary to invent an alkali-free glass fiber. Summary of the invention

[0004] In view of the above existing technical problems, the present invention aims to provide an alkali-free glass fiber and a preparation method thereof. The glass fiber prepared by this method has higher high temperature resistance, high tensile strength and small elongation, and maintains a stable shape and size; and has good chemical stability and is not easily corroded and damaged under harsh conditions such as high temperature and high humidity; and has excellent electrical insulation performance.

[0005] The present invention discloses an alkali-free glass fiber, comprising the following components in parts by weight:

[0006] Silicon dioxide 45-55%; aluminum oxide 20-30%; magnesium oxide 1-3%; calcium oxide 1.5-2%; praseodymium oxide 0.01-0.05%; wetting agent 2-3%; antioxidant 1-1.5%.

[0007] Preferably, the sizing agent is a mixture of epoxy resin, whiskers and phenolic resin.

[0008] Preferably, the mass ratio of epoxy resin to whisker is 1:(0.5-0.8).

[0009] Preferably, the mass ratio of epoxy resin to phenolic resin is 1:(1.1-1.3).

[0010] Preferably, the antioxidant is composed of 2,4-di-tert-butylphenol and bis-p-cresol in a mass ratio of 1:(0.8-1).

[0011] The present invention also discloses a method for preparing alkali-free glass fiber, comprising the following process steps:

[0012] S1 Preparation of glass melt: according to the formula design, the raw materials of silicon dioxide, aluminum oxide, magnesium oxide, calcium oxide, praseodymium oxide, infiltrant and antioxidant are weighed, mixed, and fully ground, and then placed in a high-temperature furnace for heating and melting to obtain glass melt;

[0013] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1000-1100° C. and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1500-2000 m / min to obtain glass fiber precursor.

[0014] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100° C., heating the glass fiber precursor again for continuous heat treatment, and obtaining alkali-free glass fiber after the continuous heat treatment is completed.

[0015] Preferably, in the S1 melting step, in the S1 glass melt preparation step, the heating temperature in the high temperature furnace is 1500-1700°C.

[0016] Preferably, in the S1 glass melt preparation step, the heating time in the high-temperature furnace is 1 to 2 hours.

[0017] Preferably, in the step S3 of preparing the alkali-free glass fiber, the temperature of the continuous heat treatment is 800-1000°C.

[0018] Preferably, in the step S3 of preparing the alkali-free glass fiber, the duration of the continuous heat treatment is 2 to 3 hours.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The alkali-free glass fiber provided by the present invention has high tensile strength; small elongation, stable shape and size; good chemical stability, not easy to corrode and break under harsh conditions such as high temperature and high humidity; excellent electrical insulation performance, suitable for the manufacture of electrical insulation materials; good processing performance. The alkali-free glass fiber provided by the present invention is SiO 2 -Al 2 O 3 -MgO-CaO network structure, and adding praseodymium oxide can effectively improve the stability of the network structure, increase the tensile strength and not easy to break. Adding a wetting agent to the raw materials is to make the raw materials react better and the network structure more stable.

[0021] The present invention also provides a method for preparing alkali-free glass fiber, wherein the glass melt is cooled to a slurry state before drawing, and then drawing is performed, in order to ensure that the glass fiber will not break due to excessive fluidity during the drawing process. After the drawing is completed, the temperature is first lowered, and then the temperature is raised for continuous heat treatment, because in the continuous heat treatment, the glass fiber fabric is heated at a high temperature to reduce the friction coefficient between individual fibers and improve the softness of the fabric. In addition, the continuous heat treatment can also improve the shaping of the fiber, making the fabric easier to shape. DETAILED DESCRIPTION

[0022] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0023] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0024] Embodiment 1: An alkali-free glass fiber, comprising the following components in parts by weight:

[0025] Silicon dioxide 45%; aluminum oxide 20%; magnesium oxide 1%; calcium oxide 1.5%; praseodymium oxide 0.01%; wetting agent 2%; antioxidant 1%.

[0026] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.5:1.1; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.8.

[0027] A method for preparing alkali-free glass fiber comprises the following process steps:

[0028] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1500℃ and start heating and melting. The heating reaction time is 1 hour.

[0029] After the reaction is completed, a glass melt is obtained;

[0030] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1000°C and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1500m / min to obtain glass fiber raw yarn.

[0031] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100°C, heating the glass fiber precursor to 800°C again and subjecting it to continuous heat treatment for 2 hours, alkali-free glass fiber is obtained after the continuous heat treatment is completed.

[0032] Embodiment 2: An alkali-free glass fiber, comprising the following components in parts by weight:

[0033] Silicon dioxide 47%; aluminum oxide 22%; magnesium oxide 1.5%; calcium oxide 1.6%; praseodymium oxide 0.02%; wetting agent 2.2%; antioxidant 1.1%.

[0034] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.55:1.15; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.85.

[0035] A method for preparing alkali-free glass fiber comprises the following process steps:

[0036] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1550℃ and start heating and melting. The heating reaction time is 1.2h.

[0037] After the reaction is completed, a glass melt is obtained;

[0038] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1000° C. and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1600 m / min to obtain glass fiber raw yarn.

[0039] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100°C, heating the glass fiber precursor to 850°C again and subjecting it to continuous heat treatment for 2.2h, alkali-free glass fiber is obtained after the continuous heat treatment is completed.

[0040] Embodiment 3: An alkali-free glass fiber, comprising the following components in parts by weight:

[0041] Silicon dioxide 49%; aluminum oxide 24%; magnesium oxide 2%; calcium oxide 1.7%; praseodymium oxide 0.03%; wetting agent 2.4%; antioxidant 1.2%.

[0042] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.6:1.2; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.9.

[0043] A method for preparing alkali-free glass fiber comprises the following process steps:

[0044] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1600℃ and start heating and melting. The heating reaction time is 1.4h.

[0045] After the reaction is completed, a glass melt is obtained;

[0046] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1050°C and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1700 m / min to obtain glass fiber raw yarn.

[0047] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100°C, heating the glass fiber precursor to 900°C again and subjecting it to continuous heat treatment for 2.4h, alkali-free glass fiber is obtained after the continuous heat treatment is completed.

[0048] Embodiment 4: An alkali-free glass fiber, comprising the following components in parts by weight:

[0049] Silicon dioxide 51%; aluminum oxide 26%; magnesium oxide 2.5%; calcium oxide 1.8%; praseodymium oxide 0.04%; wetting agent 2.6%; antioxidant 1.3%.

[0050] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.65:1.25; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.95.

[0051] A method for preparing alkali-free glass fiber comprises the following process steps:

[0052] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1650℃ and start heating and melting. The heating reaction time is 1.6h.

[0053] After the reaction is completed, a glass melt is obtained;

[0054] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1050°C and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1800 m / min to obtain glass fiber raw yarn.

[0055] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100°C, heating the glass fiber precursor to 950°C again and subjecting it to continuous heat treatment for 2.6h, alkali-free glass fiber is obtained after the continuous heat treatment is completed.

[0056] Embodiment 5: An alkali-free glass fiber, comprising the following components in parts by weight:

[0057] Silicon dioxide 53%; aluminum oxide 28%; magnesium oxide 3%; calcium oxide 1.9%; praseodymium oxide 0.05%; wetting agent 2.8%; antioxidant 1.4%.

[0058] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.7:1.3; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:1.

[0059] A method for preparing alkali-free glass fiber comprises the following process steps:

[0060] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1700℃ and start heating and melting. The heating reaction time is 1.8h.

[0061] After the reaction is completed, a glass melt is obtained;

[0062] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1050°C and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1900 m / min to obtain glass fiber raw yarn.

[0063] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100°C, heating the glass fiber precursor to 1000°C again and subjecting it to continuous heat treatment for 2.8h, alkali-free glass fiber is obtained after the continuous heat treatment is completed.

[0064] Embodiment 6: An alkali-free glass fiber, comprising the following components in parts by weight:

[0065] Silicon dioxide 55%; aluminum oxide 30%; magnesium oxide 3%; calcium oxide 2%; praseodymium oxide 0.05%; wetting agent 3%; antioxidant 1.5%.

[0066] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.7:1.3; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:1.

[0067] A method for preparing alkali-free glass fiber comprises the following process steps:

[0068] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1700℃ and start heating and melting. The heating reaction time is 1.8h.

[0069] After the reaction is completed, a glass melt is obtained;

[0070] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1100° C. and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 2000 m / min to obtain glass fiber raw yarn.

[0071] S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100°C, heating the glass fiber precursor to 1000°C again and subjecting it to continuous heat treatment for 3 hours, alkali-free glass fiber is obtained after the continuous heat treatment is completed.

[0072] Comparative Example 1: An alkali-free glass fiber, comprising the following components in parts by weight:

[0073] Silicon dioxide 51%; aluminum oxide 26%; magnesium oxide 2.5%; calcium oxide 1.8%; praseodymium oxide 0.04%;

[0074] Antioxidant 1.3%.

[0075] The antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:95.

[0076] The process steps and conditions of the method for preparing the alkali-free glass fiber are the same as those of Example 4.

[0077] Comparative Example 2: An alkali-free glass fiber, comprising the following components in parts by weight:

[0078] Silicon dioxide 51%; aluminum oxide 26%; magnesium oxide 2.5%; calcium oxide 1.8%; wetting agent 2.6%; antioxidant 1.3%.

[0079] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.65:1.25; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.95.

[0080] The process steps and conditions of the method for preparing the alkali-free glass fiber are the same as those of Example 4.

[0081] Comparative Example 3: An alkali-free glass fiber, comprising the following components in parts by weight:

[0082] Silicon dioxide 51%; aluminum oxide 26%; magnesium oxide 2.5%; calcium oxide 1.8%; praseodymium oxide 0.04%; wetting agent 2.6%; antioxidant 1.3%.

[0083] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.65:1.25; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.95.

[0084] A method for preparing alkali-free glass fiber comprises the following process steps:

[0085] S1 Preparation of glass melt: Mix the raw materials prepared in advance, grind them evenly, put them into a high-temperature furnace, heat them to 1650°C and start heating and melting. The heating reaction time is 1.6 hours. After the reaction is completed, a glass melt is obtained;

[0086] S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1050°C and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1800 m / min to obtain glass fiber raw yarn.

[0087] S3 Preparation of alkali-free glass fiber: The glass fiber raw yarn obtained in step S2 is cooled to 30° C. to obtain alkali-free glass fiber.

[0088] Comparative Example 4: An alkali-free glass fiber, comprising the following components in parts by weight:

[0089] Silicon dioxide 51%; aluminum oxide 26%; sodium oxide 1%; magnesium oxide 2.5%; calcium oxide 1.8%; praseodymium oxide 0.04%; wetting agent 2.6%; antioxidant 1.3%.

[0090] The impregnating agent is composed of a mixture of epoxy resin, whisker and phenolic resin in a mass ratio of 1:0.65:1.25; the antioxidant is composed of 2,4-di-tert-butylphenol and bis(p-cresol) in a mass ratio of 1:0.95.

[0091] The process steps and conditions of the glass fiber preparation method are the same as those in Example 4.

[0092] The finished glass fiber products prepared in Examples 1 to 6 and Comparative Examples 1 to 4 were tested, and the experimental data are shown in the following table:

[0093]

[0094] It can be seen from the above table that the test data from Examples 1 to 6 show that the glass fiber prepared by the method for preparing an alkali-free glass fiber provided by the present invention has high tensile strength, small expansion coefficient, small dielectric constant, high density, and excellent corrosion resistance under high temperature and high humidity environment.

[0095] Comparative Example 1 is an alkali-free glass fiber product obtained after removing the wetting agent from the raw material; Comparative Example 2 is an alkali-free glass fiber product obtained after removing praseodymium oxide from the raw material; Comparative Example 3 is an alkali-free glass fiber product obtained after continuous heat treatment in the preparation step; Comparative Example 4 is a glass fiber product obtained after adding alkali metals to the raw material. From the test data of Comparative Examples 1 to 4 and Example 4, the tensile strength and density of the glass fiber products obtained in Comparative Examples 1 to 4 will decrease, the expansion coefficient and dielectric constant will increase, and they are easily corroded in a high temperature and high humidity environment. This is because the addition of wetting agent and praseodymium oxide can promote the establishment of a network structure between the raw materials, so the performance of the obtained glass fiber product is better. Increasing continuous heating during the preparation process can reduce the friction coefficient between single fibers and improve the softness of the fabric. Adding alkali metals to the raw materials will reduce the performance of the final glass fiber product and limit the application of glass fibers.

[0096] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. An alkali-free glass fiber, characterized in that: It is composed of the following components in parts by weight: Silicon dioxide 45-55%; aluminum oxide 20-30%; magnesium oxide 1-3%; calcium oxide 1.5-2%; praseodymium oxide 0.01-0.05%; wetting agent 2-3%; antioxidant 1-1.5%.

2. The alkali-free glass fiber according to claim 1, characterized in that: The sizing agent is a mixture of epoxy resin, whisker and phenolic resin.

3. The alkali-free glass fiber according to claim 2, characterized in that: The mass ratio of the epoxy resin to the whisker is 1:(0.5-0.8).

4. The alkali-free glass fiber according to claim 2, characterized in that: The mass ratio of the epoxy resin to the phenolic resin is 1:(1.1-1.3).

5. The alkali-free glass fiber according to claim 1, characterized in that: The antioxidant is composed of 2,4-di-tert-butylphenol and bis-p-cresol in a mass ratio of 1: (0.8-1).

6. A method for preparing alkali-free glass fiber, characterized in that: The process steps include: S1 Preparation of glass melt: according to the formula design, the raw materials of silicon dioxide, aluminum oxide, magnesium oxide, calcium oxide, praseodymium oxide, infiltrant and antioxidant are weighed, mixed, and fully ground, and then placed in a high-temperature furnace for heating and melting to obtain glass melt; S2: Cooling and drawing: Cooling the glass melt prepared in step S1 to 1000-1100° C. and then starting to draw the glass melt. During the drawing process, the temperature of the glass melt is kept constant and the drawing speed is controlled to be 1500-2000 m / min to obtain glass fiber precursor. S3 preparation of alkali-free glass fiber: after cooling the glass fiber precursor obtained in step S2 to 100° C., heating the glass fiber precursor again for continuous heat treatment, and obtaining alkali-free glass fiber after the continuous heat treatment is completed.

7. The method for preparing the alkali-free glass fiber according to claim 6, characterized in that: In the S1 glass melt preparation step, the heating temperature in the high-temperature furnace is 1500-1700°C.

8. The method for preparing the alkali-free glass fiber according to claim 6, characterized in that: In the S1 glass melt preparation step, the heating time in the high-temperature furnace is 1 to 2 hours.

9. The method for preparing an alkali-free glass fiber according to claim 6, characterized in that: In the step S3 of preparing the alkali-free glass fiber, the temperature of the continuous heat treatment is 800-1000°C.

10. The method for preparing the alkali-free glass fiber according to claim 6, characterized in that: In step S3 of preparing the alkali-free glass fiber, the duration of the continuous heat treatment is 2 to 3 hours.

Citation Information

Patent Citations

  • Alkali-free glass and manufacturing technique thereof

    CN101113072A

  • Preparation method for glass fiber

    CN107032596A

  • Pr2O3-doped low-dielectric glass fibers and preparation method thereof

    CN108409150A

  • Glass fiber

    CN112759270A

  • Ecological soluble environment-friendly refractory fiber

    CN117023999A