Rocking agent for fly ash-based road, and preparation method and application thereof
The fly ash-based road lithochemical agent prepared by fly ash, slag powder and alkaline exciters solves the problems of soil shrinkage and environmental pollution in the base layer, improves the strength and stability of the base layer materials, and realizes the cost Saving and environmentally friendly roadbed treatment.
Patent Information
- Application Number
- CN202411148513.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-22
AI Technical Summary
The existing base soil modification agent has poor dry shrinkage performance and is prone to cracks, causing moisture to enter the gap to destroy the internal structure of the soil, and the production of cement and lime will cause pollution to the environment.
Fly ash based road lithochemical agent prepared with fly ash, slag powder and sheet-like alkali as exciters, small particle size substances are formed by drying, grinding and stirring, and before construction Prereacted to improve the mechanical properties of the soil.
It significantly improves the engineering mechanical strength and stability of the base material, reduces dry shrinkage and cracking, reduces production costs, is suitable for large-scale production, reduces environmental pollution, and extends the service life of the road surface.
Smart Images

Figure CN118993592A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of comprehensive utilization of industrial solid waste and road engineering materials, and specifically relates to a fly ash-based road lithification agent, a preparation method and application thereof. Background Art
[0002] With the rapid development of the national economy, the progress of engineering construction is also gradually accelerating. As an important component of construction projects, the performance of the base soil plays an important role in the quality and progress of the project. At present, in the field of highway engineering construction, the general practice of improving the soil is to add cement, lime and other curing materials into the soil to improve the engineering performance of the soil. According to years of engineering practice, traditional improvers still have many shortcomings. Cracks often appear due to shrinkage, which makes it easy for water to enter the gaps and destroy the internal structure of the soil. In addition, the production of cement and lime requires the mining of a large amount of clay, limestone, etc., which not only consumes a lot of energy, causes soil erosion and ecological imbalance, but also aggravates the deterioration of the natural environment, which is seriously contrary to the concept of ecological environment protection advocated by the country. Therefore, the existing improvers have the defects of easy shrinkage and cracks, which makes it easy for water to enter the gaps and destroy the internal structure of the soil.
[0003] Fly ash is fine dust mainly composed of glass phase, which is discharged from the flue and collected by the dust collector after the finely ground coal powder in the coal-fired power plant is burned at high temperature in the coal-fired boiler and undergoes a series of physical and chemical changes. At present, the annual emission of fly ash in my country has reached 200 million tons. Due to the poor degradation ability of fly ash, a large amount of fly ash accumulates, occupies land and pollutes the environment. Slag, also known as blast furnace slag, is a by-product of smelting pig iron in a blast furnace. As a molten product obtained from blast furnace ironmaking, it will cause harm and impact on water sources, soil and air. Therefore, preparing a material that meets various technical indicators of the base layer and can fully open up raw material channels to replace cement, lime, etc. for use in roadbed projects has become a key research direction in the field of comprehensive utilization of solid waste. Summary of the invention
[0004] The purpose of the present invention is to solve the technical problems that the existing improvers have poor shrinkage performance and are prone to cracks, which in turn causes moisture to enter the gaps and destroy the internal structure of the soil, and to provide a fly ash-based road lithification agent, a preparation method and an application.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0006] A fly ash-based road lithification agent is prepared from the following raw materials in parts by dry weight: 55 to 70 parts of fly ash, 15 to 20 parts of slag powder and 15 to 25 parts of an activator.
[0007] Furthermore, the activator is flaky powdered alkali.
[0008] A method for preparing a fly ash-based road lithification agent comprises the following steps:
[0009] S1. Detect the moisture content of each raw material of the lithification agent, calculate the wet weight ratio of each raw material according to the dry mass ratio of fly ash, slag and activator, weigh them on an electronic scale, drain them onto a conveyor belt, and enter the drying equipment together, stir and dry them to form a mixed material with a moisture content of less than 1%;
[0010] S2, feeding the mixed materials into a pulverizer and adding a grinding aid for pulverization, grinding the mixed materials to a particle size of less than 100 meshes, and obtaining a fly ash-based road rockizing agent;
[0011] S3. Put the lithification agent into a sealed packaging bag and store it at room temperature.
[0012] Furthermore, in step S2, the amount of the grinding aid is 0.05% of the weight of the mixed material, and the grinding time is 25 to 30 minutes.
[0013] An application of the fly ash-based road lithification agent comprises the following specific steps:
[0014] S1. Conduct indoor tests according to the properties of the soil used for base construction to determine the optimal dosage parameters of the lithification agent;
[0015] S2, mixing the lithification agent with soil according to the determined lithification agent dosage;
[0016] S3. After 7 days of pre-reaction, add water and mix for on-site construction.
[0017] The beneficial effects of the present invention are:
[0018] The present invention is based on the theory of depolymerization and polycondensation, the principle of geological diagenesis and the design method of geochemical engineering, that is, the reaction process in which the silicon-oxygen bonds and aluminum-oxygen bonds in the raw materials are broken and then reassembled under the action of an alkaline catalyst is taken as the basic principle. By fully activating the activity of fly ash, high-quality road lithification agents are developed to comprehensively improve the road performance.
[0019] The road-use rock-forming agent of the present invention efficiently utilizes industrial wastes such as fly ash and slag, and adopts a solid alkaline activator, which can eliminate the impact of the alkaline activator on the environment; at the same time, according to the properties of fine-grained soil, by changing the inherent chemical properties of fine-grained soil, the physical structure of the fine-grained soil can be improved and the mechanical properties can be greatly improved, thereby achieving the effects of high engineering mechanical strength and good stability; it can replace cement and lime in roadbed stabilization treatment, reduce production costs, and facilitate construction, and is suitable for road mixing method and factory mixing method construction, and is suitable for mass production.
[0020] The road lithification agent of the present invention has a micro-expansion property, can compensate for shrinkage, and prevent cracking caused by shrinkage; greatly improves the strength of the base material, and significantly enhances the fatigue resistance and durability of the base (resistance to thermal shrinkage, freeze-thaw resistance, erosion resistance, etc.); reduces dependence on sand and gravel aggregates, and significantly reduces the project cost; utilizes the strengthening effect of the lithification agent, and synergistically utilizes solid wastes such as coal gangue and construction waste to produce road base mixtures, thereby achieving waste treatment with waste.
[0021] In the roadbed stabilization treatment, the use of fly ash-based road lithification agent to replace 10,000 tons of cement and lime will reduce the emission of 5,200 to 8,000 tons of CO2 gas and save economic costs of 300,000 to 400,000 yuan. At the same time, it can extend the service life of the road surface and improve road traffic safety.
[0022] The road lithification agent of the present invention solves the technical problem that the existing improvers are easy to shrink and crack, and cause water to easily enter the gaps and destroy the internal structure of the soil. Compared with the background technology, the present invention has the advantages of saving costs, treating waste with waste, facilitating construction and prolonging the service life of the road surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a flow chart of preparing a lithogenic agent stabilized soil specimen of the present invention;
[0024] Figure 2 It is the SEM of the stabilized soil sample with a dosage of 14% in the application example of the present invention at different curing ages. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0026] Example 1
[0027] A fly ash-based road lithification agent in this embodiment is made of the following raw materials in dry weight parts: 55 parts of fly ash, 20 parts of slag powder and 25 parts of activator. The activator is flaky powdered alkali.
[0028] The main chemical compositions of the raw materials used in this example are shown in Table 1.
[0029] Table 1 Main chemical composition of raw materials (%)
[0030]
[0031] The method for preparing the fly ash-based road lithification agent in the above embodiment comprises the following steps:
[0032] S1. Detect the moisture content of each raw material of the lithification agent, calculate the wet weight ratio of each raw material according to the dry mass ratio of fly ash, slag and activator, weigh them on an electronic scale, drain them onto a conveyor belt, and enter the drying equipment together, stir and dry them to form a mixed material with a moisture content of less than 1%;
[0033] S2, feeding the mixed materials into a grinding mill and adding a grinding aid for grinding, grinding the mixed materials to a particle size of less than 100 mesh, and obtaining a fly ash-based road rockizing agent; the amount of the grinding aid is 0.05% of the weight of the mixed materials, and the grinding time is 25 to 30 minutes;
[0034] S3. Put the lithification agent into a sealed packaging bag and store it at room temperature.
[0035] Example 2
[0036] A fly ash-based road lithification agent in this embodiment is made of the following raw materials in dry weight parts: 60 parts of fly ash, 20 parts of slag powder and 20 parts of activator. The activator is flaky powdered alkali.
[0037] The main chemical components of the raw materials used in this example are the same as those in Example 1.
[0038] The preparation method of the fly ash-based road lithification agent in this embodiment is the same as that in Example 1.
[0039] Example 3
[0040] A fly ash-based road lithification agent in this embodiment is made of the following raw materials in dry weight parts: 70 parts of fly ash, 15 parts of slag powder and 15 parts of activator. The activator is flaky powdered alkali.
[0041] The main chemical components of the raw materials used in this example are the same as those in Example 1.
[0042] The preparation method of the fly ash-based road lithification agent in this embodiment is the same as that in Example 1.
[0043] In order to determine the optimal ratio for preparing the lithification agent, the present invention conducted a 7-day unconfined compressive strength test on the lithification agent prepared in the above embodiment.
[0044] Preparation of lithogenic agent stabilized soil specimens. The preparation process of lithogenic agent stabilized soil specimens is as follows: Figure 1 First, the silt is sieved, and then the fly ash-based road lithification agent prepared in Examples 1 to 3 is 10% of the weight of the silt and the sieved silt is put into a stirring pot and stirred, and then placed for 0d, 7d, 14d, 28d, and 60d, water is added to mix evenly, statically press molded, statically placed, demoulded, molded test pieces, and the test pieces are subjected to standard curing, and the 7d unconfined compressive strength of the test pieces is tested.
[0045] The unconfined compressive strength test results of Examples 1 to 3 at different placement times of 7 days are shown in Table 2.
[0046] Table 2 Test results of soil specimens stabilized by lithification agent at different placement times
[0047]
[0048] It can be seen from Table 2 that among the stabilized soil specimens prepared with lithification agents made from different raw material components, the lithification agent stabilized soil specimen obtained after pre-reaction with soil for 7 days in Example 2 has the highest 7d unconfined compressive strength, so Example 2 is selected as the optimal ratio.
[0049] Application Examples of the Invention
[0050] The specific steps of using the fly ash-based road lithification agent in the above embodiment are as follows:
[0051] S1. Conduct indoor tests according to the properties of the soil used for base construction to determine the optimal dosage parameters of the lithification agent;
[0052] The soil sample used in this embodiment is fine-grained soil excavated from a construction site in Taiyuan, Shanxi Province, which belongs to the category of silt and is low liquid limit silt. The performance parameters of the soil are shown in Table 3.
[0053] Table 3 Basic physical properties of soil
[0054]
[0055] The indoor test is as follows: the unconfined compressive strength test is carried out in accordance with the "Testing Procedures for Inorganic Binder Stabilized Materials for Highway Engineering" (JTGE51-2009), and the optimum moisture content and maximum dry density of the soil are determined by compaction test. Based on this, the unconfined compressive strength specimens of lithification agent stabilized soil with different proportions, different placement times, different dosages and different curing ages are prepared according to 98% compaction degree, and the standard curing method is adopted for curing. By changing the proportion of lithification agent, the dosage, the placement time and curing age of the specimens, the performance of lithification agent stabilized soil is comprehensively analyzed to determine the optimal dosage parameters of fly ash-based lithification agent.
[0056] The fly ash-based road lithification agent prepared in the above Example 2 was put into a stirring pot with soil in a ratio of 10%, 12%, 14%, 16%, and 18% by weight of the soil, stirred, and left for 7 days. Water was added to mix and compacted evenly, and standard curing was carried out. After the age was reached, the 7d, 28d, 60d, and 90d unconfined compressive strength of the test pieces were tested.
[0057] Comparison example
[0058] PO 42.5 cement was added to the fine-grained soil at weight percentages of 10%, 12%, 14%, 16%, and 18%, and the optimum moisture content of the mixture was determined and used to prepare the test specimens. According to the "Testing Procedures for Stabilized Materials with Inorganic Binders for Highway Engineering" (JTGE51-2009), the stabilized soil mixture was mixed evenly and pressed into shape, and then cured as required, and the unconfined compressive strength at 7d, 28d, 60d, and 90d was determined.
[0059] The test results of soil stabilized with different amounts of lithification agent at different curing ages are shown in Table 4.
[0060] Table 4 Test results of soil stabilized with different amounts of lithification agent at different curing ages
[0061]
[0062] It can be seen from the test data in Table 4 that the fly ash-based lithification agent of the present invention has obvious advantages in early strength and late strength compared with PO42.5 cement when the lithification agent dosage is ≥14%, and the 7-day unconfined compressive strength is >5.5MPa. According to the provisions of the Technical Specifications for Construction of Highway Pavement Base (JTG / T F20-2015) on base and subbase materials of different highway grades, the base should take the 7d standard curing unconfined compressive strength value of 3.5-4.5MPa, and the subbase should take 2.5-3.0MPa. Based on this, it is determined that the optimal dosage of stabilized silt as the base or subbase lithification agent is ≥14%.
[0063] Figure 2 The present invention uses fly ash-based road lithification agent with a dosage of 14% and the SEM photos of stabilized soil samples magnified 10,000 times after 7 days, 28 days, 60 days and 90 days. The lithification agent and fine-grained soil were mixed and pre-reacted for 7 days to prepare the stabilized soil specimens. From the samples cured for 7 days, the produced calcium silicate aluminate hydrate (C-A-S-H) gel was observed to mainly show flocculent structure and snowflake structure. At the same time, some calcium aluminate hydrate (C-A-H) products were also observed, and their microstructure was mainly strip-shaped. However, the formed gelling material has not yet filled the surface of the soil particles densely, there are a large number of pores, and the structure is loose. When the curing age of the sample exceeds 28 days, there are obvious polymer crystal components on the surface of the sample, mainly including calcium silicate aluminate hydrate (C-A-S-H), calcium aluminate hydrate (C-A-H), calcium sulfonate (AFt) and sodium silicate aluminate hydrate (N-A-S-H). Its microstructure is mainly block-shaped, flake-shaped and rod-shaped. The hydration products and soil particles are intertwined to form a spatial grid structure, thereby improving the overall strength and stability. With the extension of curing time, these hydration products react more fully, the pores on the surface of the 60d sample have been greatly reduced, and its density has increased. On the microscopic surface of the 90d sample, a large number of particles have been cemented, and the pores have been filled, forming a relatively flat surface with improved strength.
[0064] S2, mixing the lithification agent with soil according to the determined lithification agent dosage;
[0065] S3. After 7 days of pre-reaction, add water and mix for on-site construction.
[0066] In order to demonstrate the use effect of the fly ash-based road lithification agent of the present invention, a road section test was carried out on the lithification agent prepared in the above Example 2, and the test results are as follows.
[0067] Test section: Take the test section for construction and follow-up observation. The specific situation is as follows:
[0068] The technical indicators of physical properties of soil at the construction site are shown in Table 5.
[0069] Table 5 Basic physical properties technical indicators of test section soil
[0070]
[0071] Judging from the test index, the soil used in this project is low liquid limit silt.
[0072] The paving position of the test road is 30 to 80 cm from the top of the roadbed. The paving plan is divided into three test sections. The lithification agent dosage is 14% and 18%, and the pre-reaction time is 7 days for the lithification agent stabilized soil.
[0073] The control example was constructed using cement stabilized soil with a cement content of 6%.
[0074] The unconfined compressive strength, compaction and deflection of the test section were tested, and the obtained parameters are shown in Table 6.
[0075] Table 6 Test section performance test
[0076]
[0077] The core samples of the test section were tested, and the test results are shown in Table 6. The mechanical strength of the test section fully meets the design strength requirements of the "Technical Specifications for Construction of Engineering Pavement Base" (JTJ034-2000); the compaction degree meets the standard requirement of not less than 96%; the deflection value of the stabilized soil is much lower than that of cement stabilized soil, and the improvement effect of the lithification agent on the bearing capacity of the roadbed and the elastic modulus of the stabilized soil layer is significantly better than that of lime soil. Further follow-up observations were conducted on the strength of the above test section. After one year of follow-up observations, the road surface of the section within the test range was smooth, without subsidence and rutting, and no longitudinal, transverse and reflective cracks appeared.
[0078] The above specific embodiments are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the following description, and these obvious changes or modifications based on the spirit of the present invention are still within the scope of protection of the present invention.
Claims
1. A fly ash-based road lithification agent, characterized in that: The invention is prepared from the following raw materials in dry weight parts: 55-70 parts of fly ash, 15-20 parts of slag powder and 15-25 parts of activator.
2. A fly ash-based road lithification agent according to claim 1, characterized in that: The activator is flaky powdered alkali.
3. A method for preparing the fly ash-based road lithification agent according to claim 1, characterized in that: The steps include: S1. Detect the moisture content of each raw material of the lithification agent, calculate the wet weight ratio of each raw material according to the dry mass ratio of fly ash, slag and activator, weigh them on an electronic scale, drain them onto a conveyor belt, and enter the drying equipment together, stir and dry them to form a mixed material with a moisture content of less than 1%; S2, feeding the mixed materials into a pulverizer and adding a grinding aid for pulverization, grinding the mixed materials to a particle size of less than 100 meshes, and obtaining a fly ash-based road rockizing agent; S3. Put the lithification agent into a sealed packaging bag and store it at room temperature.
4. The preparation method according to claim 3, characterized in that: In step S2, the amount of the grinding aid is 0.05% of the weight of the mixed materials, and the grinding time is 25 to 30 minutes.
5. An application of the fly ash-based road lithification agent according to claim 1, characterized in that: The specific steps are: S1. Conduct indoor tests according to the properties of the soil used for base construction to determine the optimal dosage parameters of the lithification agent; S2, mixing the lithification agent with soil according to the determined lithification agent dosage; S3. After 7 days of pre-reaction, add water and mix for on-site construction.
Citation Information
Cited By
Fly ash-based low-carbon cementing material acting on highway semi-rigid base
CN122233744A