Early strength agent of solid waste cementing material as well as preparation method and application of early strength agent

By using early strength agents such as potassium hydroxide, titanium dioxide, sodium metaaluminate and potassium dihydrogen phosphate in solid waste gelling materials, the problem of insufficient strength in the early stage of solid waste gelling materials was solved, and the early stage was significantly improved. Strength and flexibility to adjust the coagulation and hardening speed.

CN118993603APending Publication Date: 2024-11-22ANHUI CHENGHONGJIAN NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411112882.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Solid waste gelling materials show insufficient flexible matching capabilities in mine filling projects with high early strength requirements, and the traditional early strength agent is not very suitable.

Method used

Provide a premature enhancement agent for solid waste gelling material, including potassium hydroxide, titanium dioxide, sodium metaaluminate, potassium dihydrogen phosphate and sodium citrate. Through uniform mixing and dispersion of these components, a nano-scale dispersion liquid is formed. , added to solid waste gelling material to improve its early strength.

Benefits of technology

The early strength of solid waste gelling materials is significantly improved, and the coagulation and hardening speed can be adjusted by adjusting the amount of early strength agent added to meet different application needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of binding material additives, and discloses an early strength agent of a solid waste binding material as well as a preparation method and application of the early strength agent. The early strength agent of the solid waste cementing material comprises the following components in parts by weight: 5-10 parts of potassium hydroxide, 3-7 parts of titanium dioxide, 8-12 parts of sodium metaaluminate, 8-12 parts of monopotassium phosphate, 8-12 parts of sodium citrate and water. According to the early strength agent provided by the invention, under the matching action of potassium hydroxide, titanium dioxide, sodium metaaluminate, monopotassium phosphate and sodium citrate, the early strength agent is added into the solid waste cementing material, so that the effect of well improving the early strength of the solid waste cementing material can be achieved. Besides, according to use requirements, the setting and hardening speed of the solid waste cementing material can be adjusted by adjusting the addition amount of the early strength agent in the solid waste cementing material, so that the requirements of enterprises such as mixing plants, engineering companies and prefabricated parts are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cementitious material additives, and in particular to an early strength agent for solid waste cementitious materials and a preparation method and application thereof. Background Art

[0002] Solid waste cementitious materials are hydraulic cementitious materials made from industrial solid wastes such as blast furnace slag, desulfurized gypsum, and fly ash as the main raw materials. From the perspective of material properties, solid waste cementitious materials are structural skeletons based on calcium sulfonate and hydrated calcium silicate. They have the characteristics of low hydration heat, micro-expansion, and strong resistance to sulfate erosion. They can effectively alleviate the surface shrinkage and cracking caused by the temperature difference between day and night. From the perspective of production technology, no clinker needs to be added to solid waste cementitious materials, and the production process only requires "one grinding". Compared with traditional silicate cement, the production process is simple, eliminating the need for "one grinding and one burning", which can effectively reduce production carbon emissions and has significant social and economic benefits.

[0003] Cement as a filling cementitious material has problems such as high carbon emissions, sensitivity to sulfides, and high prices. Compared with cement, solid waste cementitious materials are not only energy-saving and environmentally friendly, but also suitable for whole tailings, graded tailings, and ultra-fine tailings. While meeting the requirements, they are also low-priced.

[0004] For mine filling projects with high requirements for early strength (1d, 3d), the requirements for early strength of mine filling projects cannot be flexibly matched by solid waste cementitious materials alone.

[0005] The main function of traditional early strength agents is to improve the early strength of concrete. They are mainly divided into chloride series, sulfate series, and organic series. The main principle is to react with C in cement to improve the early strength of concrete. 3 A acts to generate hydrated chloroaluminate which is insoluble in water and can accelerate the C 3 A hydration. Or react with calcium hydroxide produced by cement hydration to produce extremely fine particles and highly active calcium sulfate, which accelerates C 3 A is the rate at which reaction produces calcium sulphoaluminate hydrate.

[0006] However, the strength source of solid waste cementitious materials mainly comes from CSH gel and Aft, which is different from cement. The applicability of traditional early strength agents is not high.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The object of the present invention is to provide an early strength agent for solid waste gelling materials and a preparation method and application thereof, aiming to improve at least one of the problems mentioned in the background technology.

[0009] The present invention is achieved in that:

[0010] In a first aspect, the present invention provides an early strength agent for solid waste gelling materials, which comprises, by weight:

[0011] 5-10 parts of potassium hydroxide, 3-7 parts of titanium dioxide, 8-12 parts of sodium aluminate and 8-12 parts of potassium dihydrogen phosphate, 8-12 parts of sodium citrate and 50-70 parts of water.

[0012] In an alternative embodiment, the titanium dioxide is a nanoscale material.

[0013] In a second aspect, the present invention provides a method for preparing an early strength agent according to any one of the aforementioned embodiments, comprising uniformly mixing the components.

[0014] In an optional embodiment, the manner of uniformly mixing the components includes:

[0015] The components are dispersed in water to obtain respective dispersions, and the respective dispersions are mixed evenly.

[0016] In an optional embodiment, the manner of uniformly mixing the components includes:

[0017] Mixing nano-potassium titanate with water to generate a first dispersion containing potassium hydroxide and nano-titanium dioxide;

[0018] Mixing sodium aluminate and water and dispersing them uniformly to obtain a second dispersion liquid in which sodium aluminate is dispersed;

[0019] Mixing potassium dihydrogen phosphate and water and dispersing them uniformly to obtain a third dispersion liquid in which potassium dihydrogen phosphate is dispersed;

[0020] Mixing sodium citrate and water and dispersing them uniformly to obtain a fourth dispersion liquid in which sodium citrate is dispersed;

[0021] The first dispersion liquid, the second dispersion liquid, the third dispersion liquid, and the fourth dispersion liquid are mixed.

[0022] In a third aspect, the present invention provides application of the above-mentioned early strength agent in solid waste cementitious materials.

[0023] The present invention has the following beneficial effects:

[0024] An early strength agent for solid waste gelling material provided by an embodiment of the present invention, wherein potassium hydroxide in the early strength agent is used to increase the pH value of the solid waste gelling material. In a high pH environment, calcium silicate (C 3 S) hydration reaction produces more CSH gel and Ca(OH) 2 , so that C 3A is more likely to react with water to generate calcium sulfoxide (Aft) and hydrated calcium aluminate (Afm), which improves early strength; titanium dioxide, as a filling material, can fill the pores in the cement paste and improve the density and strength of the material; TiO 2 The particles can serve as nucleation points for hydration products, promote the formation of CSH gel, and accelerate the hydration reaction rate; sodium aluminate can provide aluminum ions to promote the formation of Aft (ettringite), thereby improving the early strength of the material; potassium dihydrogen phosphate can provide phosphate ions to further promote the formation of Aft and enhance the early strength; sodium citrate can create a stable and uniform reaction environment by adjusting the pH value, complexing calcium ions, and improving dispersibility, which is conducive to the uniform distribution and reaction of the early strength agent and promotes the C in the cement paste. 3 S and C 3 The uniform hydration reaction of A generates uniform CSH gel and ettringite, which improves the early strength; the addition of water disperses the effective ingredients of the early strength agent in advance, and after being added to the cementitious material, the dispersion uniformity of the various components in the early strength agent can be better.

[0025] Therefore, the early strength agent provided by the present invention, under the coordinated action of potassium hydroxide, titanium dioxide, sodium aluminate, potassium dihydrogen phosphate and sodium citrate, is added to the solid waste cementitious material to play a good role in increasing the early strength of the solid waste cementitious material. In addition, according to the use requirements, the coagulation and hardening speed of the solid waste cementitious material can be adjusted by adjusting the amount of the early strength agent added to the solid waste cementitious material, thereby meeting the needs of enterprises such as mixing stations, engineering companies, and prefabricated components. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0027] The characteristics and performance of the early strength agent for solid waste gelling materials provided by the present invention, as well as the preparation method and application thereof, are further described in detail below in conjunction with the embodiments.

[0028] An early strength agent for solid waste gelling materials provided in an embodiment of the present invention comprises, by weight:

[0029] 5-10 parts of potassium hydroxide, 3-7 parts of titanium dioxide, 8-12 parts of sodium aluminate and 8-12 parts of potassium dihydrogen phosphate, 8-12 parts of sodium citrate and water.

[0030] Potassium hydroxide in the early strength agent is a strong alkali, which will increase the pH value of the cement paste and help accelerate the formation of calcium silicate (C3 S) and calcium aluminate (C 3 A) hydration reaction; in a high pH environment, calcium silicate (C 3 S) hydration reaction produces more CSH gel and Ca(OH) 2 , improve early strength; in a high pH environment, C 3 A reacts more easily with water to form ettringite (Aft) and hydrated calcium aluminate (Afm), which improves early strength.

[0031] Titanium dioxide, as a filling material, can fill the pores in cement paste and improve the density and strength of the material; TiO 2 The particles can serve as nucleation points for hydration products, promote the formation of CSH gel, and accelerate the hydration reaction.

[0032] Sodium aluminate can provide aluminum ions and promote the formation of Aft (ettringite), thereby improving the early strength of the material.

[0033] Potassium dihydrogen phosphate can provide phosphate ions to further promote the formation of Aft and enhance early strength.

[0034] Citrate ion (C 6 H 5 O 7 3- ) can combine with hydrogen ions (H+) in the system to play a buffering role, prevent the pH value from being too high or too low, and maintain the stability of the reaction environment. By controlling the pH value within the appropriate range of 9-11 through the buffering effect, it can promote the reaction of calcium silicate (C 3 The hydration of CSH gel can also prevent calcium ions from precipitating too quickly under high alkaline conditions. 6 H 5 O 7 3- ) has a strong chelating ability and can complex the calcium ions (Ca 2 +), forming a stable complex. By complexing calcium ions, sodium citrate can prevent calcium ions from precipitating too quickly under high pH conditions, maintain a stable concentration of calcium ions, and promote the uniform formation of hydration products (such as CSH gel and calcium aluminate); complexing calcium ions can also prevent the premature formation of insoluble calcium compounds, thereby ensuring a continuous supply of calcium ions in the system, which is beneficial to the improvement of early strength; the presence of sodium citrate can also improve the dispersibility of the components in the early strength agent, prevent the agglomeration of other ingredients (such as nano-scale titanium dioxide), and ensure the uniform distribution of the components in the system. Therefore, sodium citrate can create a stable and uniform reaction environment by adjusting the pH value, complexing calcium ions, and improving dispersibility, which is conducive to the uniform distribution and reaction of the early strength agent and promotes the C in the cement paste. 3S and C 3 The uniform hydration reaction of A generates uniform CSH gel and ettringite, which improves the early strength; the addition of water disperses the effective ingredients of the early strength agent in advance, and after being added to the cementitious material, the dispersion uniformity of the various components in the early strength agent can be better.

[0035] The early strength agent provided by the present invention, under the coordinated action of potassium hydroxide, titanium dioxide, sodium aluminate, potassium dihydrogen phosphate and sodium citrate, is added to the solid waste cementitious material to play a good role in increasing the early strength of the solid waste cementitious material. In addition, according to the use requirements, the coagulation and hardening speed of the solid waste cementitious material can be adjusted by adjusting the amount of the early strength agent added to the solid waste cementitious material, so as to meet the mine filling requirements.

[0036] Optionally, titanium dioxide is a nano-scale material. Nano titanium dioxide particles have a high specific surface area and high reactivity, can promote hydration reactions, and improve early strength; and under the action of sodium citrate, the nano-scale particles can be more evenly dispersed in the system.

[0037] The preparation method of the early strength agent provided in the embodiment of the present invention comprises: uniformly mixing the components thereof.

[0038] Specifically, the components are dispersed in water to obtain respective dispersions, and the respective dispersions are mixed evenly.

[0039] You can also:

[0040] Mixing nano-potassium titanate with water to generate a first dispersion containing potassium hydroxide and nano-titanium dioxide;

[0041] Mixing sodium aluminate and water and dispersing them uniformly to obtain a second dispersion liquid in which sodium aluminate is dispersed;

[0042] Mixing potassium dihydrogen phosphate and water and dispersing them uniformly to obtain a third dispersion liquid in which potassium dihydrogen phosphate is dispersed;

[0043] Mixing sodium citrate and water and dispersing them uniformly to obtain a fourth dispersion liquid in which sodium citrate is dispersed;

[0044] The first dispersion, the second dispersion, the third dispersion and the fourth dispersion are mixed to obtain an early strength agent.

[0045] The application of the early strength agent provided in the embodiment of the present invention in the solid waste gel material. When the early strength agent is applied to the solid waste gel material, the early strength of the solid waste gel material can be significantly improved.

[0046] Specifically, the solid waste gelling material includes, by weight:

[0047] 38.5 to 49.5 parts of mineral powder, 21 to 27 parts of the solid waste material, 10.5 to 3.5 parts of gypsum and 10 to 30 parts of the early strength agent. Optionally, the solid waste material is steel slag.

[0048] The method for preparing the solid waste gelling material provided by the embodiment of the present invention comprises mixing the raw materials of various components uniformly.

[0049] Example 1

[0050] This embodiment provides an early strength agent and a solid waste gelling material containing the early strength agent.

[0051] The early strength agent includes by weight:

[0052] 7 parts of potassium hydroxide, 5 parts of titanium dioxide, 10 parts of sodium aluminate, 10 parts of potassium dihydrogen phosphate, 10 parts of sodium citrate and 65 parts of water.

[0053] Solid waste cementitious materials include by weight:

[0054] 44 parts of S95 grade mineral powder, 24 parts of first-grade steel slag powder, 12 parts of gypsum with a grade of >70%, and 20 parts of early strength agent.

[0055] Example 2

[0056] This embodiment provides an early strength agent and a solid waste gelling material containing the early strength agent.

[0057] The early strength agent includes by weight:

[0058] 8 parts of potassium hydroxide, 4 parts of titanium dioxide, 8 parts of sodium aluminate, 12 parts of potassium dihydrogen phosphate, 8 parts of sodium citrate and 60 parts of water.

[0059] Solid waste cementitious materials include by weight:

[0060] 41.25 parts of S95 grade mineral powder, 22.5 parts of first-grade steel slag powder, 11.25 parts of gypsum with a grade of >70%, 75 parts of high silicate solid waste (diatomaceous earth), and 25 parts of early strength agent.

[0061] Example 3

[0062] This embodiment provides an early strength agent and a solid waste gelling material containing the early strength agent.

[0063] The early strength agent includes by weight:

[0064] 9 parts of potassium hydroxide, 6 parts of titanium dioxide, 12 parts of sodium aluminate, 8 parts of potassium dihydrogen phosphate, 12 parts of sodium citrate and 70 parts of water.

[0065] Solid waste cementitious materials include by weight:

[0066] 38.5 parts of S95 grade mineral powder, 21 parts of first-grade steel slag powder, 10.5 parts of gypsum with a grade of >70%, and 30 parts of early strength agent.

[0067] Example 4

[0068] This embodiment provides an early strength agent and a solid waste gelling material containing the early strength agent.

[0069] The early strength agent includes by weight:

[0070] 10 parts of potassium hydroxide, 7 parts of titanium dioxide, 12 parts of sodium aluminate, 12 parts of potassium dihydrogen phosphate, 12 parts of sodium citrate and 50 parts of water.

[0071] Solid waste cementitious materials include by weight:

[0072] 49.5 parts of S95 grade mineral powder, 27 parts of first-grade steel slag powder, 13.5 parts of gypsum with a grade of >70%, and 10 parts of early strength agent.

[0073] Comparative Example 1

[0074] This comparative example is substantially the same as Example 1, except that potassium hydroxide is not included in the early strength agent; and the potassium hydroxide in Example 1 is replaced by an equal amount of sodium citrate.

[0075] Comparative Example 2

[0076] This comparative example is substantially the same as Example 1, except that the early strength agent does not include titanium dioxide.

[0077] Comparative Example 3

[0078] This comparative example is basically the same as Example 1, except that the early strength agent does not include sodium aluminate; and the sodium aluminate in Example 1 is replaced by an equal amount of potassium dihydrogen phosphate.

[0079] Comparative Example 4

[0080] This comparative example is basically the same as Example 1, except that potassium dihydrogen phosphate is not included in the early strength agent; and the potassium dihydrogen phosphate in Example 1 is replaced by an equal amount of sodium aluminate.

[0081] Comparative Example 5

[0082] This comparative example is substantially the same as Example 1, except that the early strength agent does not include sodium citrate; and the sodium citrate in Example 1 is replaced by an equal amount of potassium hydroxide.

[0083] Experimental example

[0084] The performance of the solid waste gelling materials provided in the test examples and comparative examples was tested by the following method:

[0085] Molding test pieces: Mix each component of the solid waste gel material with water to form a slurry, pour the slurry into a mold, and mold the test piece.

[0086] Curing: Curing the specimens under standard conditions (temperature 20±2℃, relative humidity above 95%).

[0087] Compression strength test: Compression strength test was carried out at different ages (3 days, 7 days, 28 days).

[0088] The test standard is based on the "Standard for Test Methods of Mechanical Properties of Ordinary Concrete" (GB / T 50081-2019). The test results are recorded in Table 1.

[0089] Table 1 Properties of solid waste cementitious materials of various embodiments and comparative examples

[0090] Group 3d / Mpa 7d / Mpa 28d / Mpa Slurry pH Example 1 27.00 40.00 52.00 10.2 Example 2 27.26 41.19 53.69 10.5 Example 3 28.56 43.32 55.08 10.8 Example 4 29.85 44.59 56.70 11.0 Comparative Example 1 20.77 30.58 45.36 9.2 Comparative Example 2 22.07 33.12 47.03 9.5 Comparative Example 3 23.36 35.67 48.60 9.7 Comparative Example 4 24.66 38.22 50.22 9.9 Comparative Example 5 25.96 39.49 51.03 10.1

[0091] It can be seen from Table 1 that the solid waste cementitious materials provided by various embodiments of the present invention have better early strength.

[0092] Comparing each comparative example with Example 1, the early strength of each comparative example is significantly worse than that of Example 1, which indicates that the early strength agent provided by the present invention can significantly improve the early strength of the solid waste cementitious material, and the lack of any component in the early strength agent will cause the early strength to decrease.

[0093] In summary, the early strength agent provided by the present invention, under the coordinated action of potassium hydroxide, titanium dioxide, sodium aluminate, potassium dihydrogen phosphate and sodium citrate, is added to the solid waste cementitious material to play a good role in increasing the early strength of the solid waste cementitious material.

[0094] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An early strength agent for solid waste gelling materials, characterized in that: The components include by weight: 5-10 parts of potassium hydroxide, 3-7 parts of titanium dioxide, 8-12 parts of sodium aluminate and 8-12 parts of potassium dihydrogen phosphate, 8-12 parts of sodium citrate and 50-70 parts of water.

2. The early strength agent according to claim 1, characterized in that Titanium dioxide is a nanoscale material.

3. A method for preparing the early strength agent according to claim 1 or 2, characterized in that: Including mixing the components evenly.

4. The preparation method according to claim 3, characterized in that: Methods for mixing the components uniformly include: The components are dispersed in water to obtain respective dispersions, and the respective dispersions are mixed evenly.

5. The preparation method according to claim 3, characterized in that: Methods for mixing the components uniformly include: Mixing nano-potassium titanate with water to generate a first dispersion containing potassium hydroxide and nano-titanium dioxide; Mixing sodium aluminate and water and dispersing them uniformly to obtain a second dispersion liquid in which sodium aluminate is dispersed; Mixing potassium dihydrogen phosphate and water and dispersing them uniformly to obtain a third dispersion liquid in which potassium dihydrogen phosphate is dispersed; Mixing sodium citrate and water and dispersing them uniformly to obtain a fourth dispersion liquid in which sodium citrate is dispersed; The first dispersion liquid, the second dispersion liquid, the third dispersion liquid, and the fourth dispersion liquid are mixed.

6. Use of the early strength agent as claimed in claim 1 or 2 in solid waste gel material.

Citation Information

Cited By

  • Method for improving early-stage performance of all-solid waste cementing material

    CN120829290A